打印参数对电子束增材制造Ti-Ni合金性能的影响
任德春1,2, 张慧博1, 赵晓东3, 王福雨4, 侯文韬1, 王绍钢1, 李述军1, 金伟1(), 杨锐1
1 中国科学院金属研究所 沈阳 110016
2 中国科学技术大学材料科学与工程学院 沈阳 110016
3 东北大学材料科学与工程学院材料各向异性与织构教育部重点实验室 沈阳 110819
4 中国航空工业集团公司沈阳飞机设计研究所 沈阳 110035
Influence of Manufacturing Parameters on the Properties of Electron Beam Melted Ti-Ni Alloy
REN Dechun1,2, ZHANG Huibo1, ZHAO Xiaodong3, WANG Fuyu4, HOU Wentao1, WANG Shaogang1, LI Shujun1, JIN Wei1(), YANG Rui1
1 Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
2 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
3 Key Laboratory for Anisotropy and Texture of Materials (Ministry of Education), School of Materials Science and Engineering, Northeastern University, Shenyang 110819, China
4 AVIC Shenyang Aircraft Design and Research Institute, Shenyang 110035, China
引用本文:

任德春, 张慧博, 赵晓东, 王福雨, 侯文韬, 王绍钢, 李述军, 金伟, 杨锐. 打印参数对电子束增材制造Ti-Ni合金性能的影响[J]. 金属学报, 2020, 56(8): 1103-1112.
Dechun REN, Huibo ZHANG, Xiaodong ZHAO, Fuyu WANG, Wentao HOU, Shaogang WANG, Shujun LI, Wei JIN, Rui YANG. Influence of Manufacturing Parameters on the Properties of Electron Beam Melted Ti-Ni Alloy[J]. Acta Metall Sin, 2020, 56(8): 1103-1112.

全文: PDF(3792 KB)   HTML
摘要: 

利用SEM、XRD、DSC、TEM和等轴压缩等实验手段,研究和分析了打印参数焦距补偿(FO)和速度函数(SF)对电子束增材制造(EBM)制备的Ti-Ni合金显微组织、相组成、相变行为以及压缩性能的影响。结果表明:EBM打印参数FO和SF在一定范围内调节时均可制备出相对密度较高(97%以上)的Ti-Ni合金样品。由于EBM电子束的功率大,在预合金粉末快速受热熔化过程中,Ni元素的挥发效应大于富Ti相Ti2Ni析出效应对相变温度的影响,使得制备Ti-Ni块体的相变温度大于相应的预合金粉末,而打印参数FO和SF对制备样品的相变温度、相组成以及显微硬度的影响较小。EBM制备过程中在样品内部引入不同种类的缺陷类型,使得Ti-Ni合金样品在相对密度接近的情况下压缩性能表现出极大的差异,其中贯穿型裂纹缺陷对压缩性能的影响最大,使Ti-Ni合金的强度和塑性大幅度降低。

关键词 : 电子束增材制造,  Ti-Ni合金,  制备参数,  显微组织,  压缩性能    
Abstract:

Electron beam melting (EBM) is one of the additive manufacturing technologies which can be used to fabricate the complex structure and shape samples. Until now, there are few literatures published about the properties of Ti-Ni samples produced by EBM. In this work, the influence of two important manufacturing parameters of focus offset (FO) and speed function (SF) on the density, phase content and transformation behavior, microstructure and mechanical properties was investigated for the equiatomic Ti-Ni shape memory alloy fabricated by EBM used DSC, XRD, SEM, TEM and electronic universal testing machine. The results showed that all the Ti-Ni samples had a high relative density beyond than 97% for fabricated by different combinations of FO and SF in the selected range. The corresponding phase transformation temperatures for all the Ti-Ni samples fabricated by EBM were higher than the pre-alloyed Ti-Ni powder, due to the effect of evaporation of Ni element higher than that of the formation of Ni-rich Ti2Ni phase during the quickly melting and solidification process. On the other hand, the EBM manufacturing parameters of FO and SF had limited influence on the phase contents, phase transformation temperatures and Vickers hardness. Due to the feature of the EBM fabricating method, the different types of defects would be introduced in the Ti-Ni solid samples. Though all the samples had similar high relative density, the performance of the compression behavior were shown great difference, and the crack defect had the larger effect than the gas and lack-of fusion porosities on the compression fracture stress and strain.

Key words: electron beam melting    Ti-Ni alloy    manufacturing parameter    microstructure    compression property
收稿日期: 2019-11-29     
ZTFLH:  TG146.23  
基金资助:中国科学院战略性先导科技专项(A类)项目(XDA22010103)
作者简介: 任德春,男,1991年生,博士生
SampleSF / (mm·s-1)FO / mA
S1258
S22515
S32535
S42540
S57015
S68015
S710015
表1  电子束增材制造(EBM)制备Ti-Ni合金具体参数
图1  电子束增材制造(EBM)用Ti-Ni预合金粉末形貌的SEM像
图2  不同EBM打印参数制备的Ti-Ni合金样品的实测密度和相对密度
图3  Ti-Ni预合金粉末和不同EBM打印参数制备的Ti-Ni合金样品的XRD谱
图4  Ti-Ni预合金粉末和EBM制备Ti-Ni合金样品的DSC曲线
SampleMfMpMsAsApAf
Powder24.8/52.530.8/54.637.1/57.558.1/72.764.9/76.770.9/83.5
S145.558.470.776.692.8103.9
S247.660.972.179.395.1104.8
S341.355.569.773.089.0102.0
S435.657.672.374.390.6101.4
S549.461.573.581.195.8107.0
S648.360.972.282.695.9105.3
S748.661.072.482.495.3105.3
表2  Ti-Ni预合金粉末和EBM 制备Ti-Ni合金样品的相变温度 (℃)
图5  EBM制备Ti-Ni合金样品的室温压缩应力-应变曲线
图6  EBM制备不同Ti-Ni合金样品的显微硬度及样品S5沿打印方向平面和打印平面上表面的显微硬度
图7  EBM制备不同Ti-Ni合金样品的显微组织
图8  EBM制备Ti-Ni合金样品S5的表面形貌、显微组织和EDS分析
图9  EBM制备Ti-Ni合金样品S5显微组织的TEM 像和SAED谱
图10  EBM 制备Ti-Ni合金样品的缺陷分析
[1] Jiang H C, Rong L J. Releasing behavior of Ni in porous NiTi shape memory alloy [J]. Acta Metall. Sin., 2008, 44: 198
[1] (姜海昌, 戎利建. 多孔NiTi形状记忆合金中Ni的释放行为 [J]. 金属学报, 2008, 44: 198)
[2] He Z R, Wu P Z, Liu K K, et al. Microstructure, phase transformation and shape memory behavior of chilled Ti-47Ni alloy ribbons [J]. Acta Metall. Sin., 2018, 54: 1157
doi: 10.11900/0412.1961.2017.00410
[2] (贺志荣, 吴佩泽, 刘康凯等. 激冷Ti-47Ni合金薄带的组织、相变和形状记忆行为 [J]. 金属学报, 2018, 54: 1157)
doi: 10.11900/0412.1961.2017.00410
[3] Liu X P, Jin W, Meng C G, et al. Effect of cold deformation on the transformation behaviors of TiNi film [J]. Acta Metall. Sin., 2001, 37: 589
[3] (刘晓鹏, 金 伟, 孟长功等. 预变形对TiNi薄膜相变行为的影响 [J]. 金属学报, 2001, 37: 589)
[4] Elahinia M H, Hashemi M, Tabesh M, et al. Manufacturing and processing of NiTi implants: A review [J]. Prog. Mater. Sci., 2012, 57: 911
doi: 10.1016/j.pmatsci.2011.11.001
[5] Liu L J, Li S J, Wang H L, et al. Microstructure, defects and mechanical behavior of beta-type titanium porous structures manufactured by electron beam melting and selective laser melting [J]. Acta Mater., 2016, 113: 56
doi: 10.1016/j.actamat.2016.04.029
[6] Zhao X L, Li S J, Zhang M, et al. Comparison of the microstructures and mechanical properties of Ti-6Al-4V fabricated by selective laser melting and electron beam melting [J]. Mater. Des., 2016, 95: 21
doi: 10.1016/j.matdes.2015.12.135
[7] Ren D C, Li S J, Wang H, et al. Fatigue behavior of Ti-6Al-4V cellular structures fabricated by additive manufacturing technique [J]. J. Mater. Sci. Technol., 2019, 35: 285
[8] Wang C C, Tan X P, Liu E J, et al. Process parameter optimization and mechanical properties for additively manufactured stainless steel 316L parts by selective electron beam melting [J]. Mater. Des., 2018, 147: 157
doi: 10.1016/j.matdes.2018.03.035
[9] Wang P, Sin W J, Nai M L S, et al. Effects of processing parameters on surface roughness of additive manufactured Ti-6Al-4V via electron beam melting [J]. Materials, 2017, 10: 1121
doi: 10.3390/ma10101121
[10] Zhang L C, Liu Y J, Li S J, et al. Additive manufacturing of titanium alloys by electron beam melting: A review [J]. Adv. Eng. Mater., 2018, 20: 1700842
doi: 10.1002/adem.v20.5
[11] Pushilina N, Syrtanov M, Kashkarov E, et al. Influence of manufacturing parameters on microstructure and hydrogen sorption behavior of electron beam melted titanium Ti-6Al-4V alloy [J]. Materials, 2018, 11: 763
doi: 10.3390/ma11050763
[12] Saedi S, Turabi A S, Andani M T, et al. The influence of heat treatment on the thermomechanical response of Ni-rich NiTi alloys manufactured by selective laser melting [J]. J. Alloys Compd., 2016, 677: 204
doi: 10.1016/j.jallcom.2016.03.161
[13] Ma J, Franco B, Tapia G, et al. Spatial control of functional response in 4D-Printed active metallic structures [J]. Sci. Rep., 2017, 7: 46707
doi: 10.1038/srep46707 pmid: 28429796
[14] Moghaddam N S, Saghaian S E, Amerinatanzi A, et al. Anisotropic tensile and actuation properties of NiTi fabricated with selective laser melting [J]. Mater. Sci. Eng., 2018, A724: 220
[15] Habijan T, Haberland C, Meier H, et al. The biocompatibility of dense and porous nickel-titanium produced by selective laser melting [J]. Mater. Sci. Eng., 2013, C33: 419
[16] Li S, Hassanin H, Attallah M M, et al. The development of TiNi-based negative Poisson's ratio structure using selective laser melting [J]. Acta Mater., 2016, 105: 75
doi: 10.1016/j.actamat.2015.12.017
[17] Ren D C, Zhang H B, Liu Y J, et al. Microstructure and properties of equiatomic Ti-Ni alloy fabricated by selective laser melting [J]. Mater. Sci. Eng., 2020, A771: 138586
[18] Hayat M D, Chen G, Khan S, et al. Physical and tensile properties of NiTi alloy by selective electron beam melting [J]. Key Eng. Mater., 2018, 770: 148
doi: 10.4028/www.scientific.net/KEM.770
[19] Schwerdtfeger J, Singer R F, Körner C. In situ flaw detection by IR-imaging during electron beam melting [J]. Rapid Prototyp. J., 2012, 18: 259
doi: 10.1108/13552541211231572
[20] Al-Bermani S S. An investigation into microstructure and microstructural control of additive layer manufactured Ti-6Al-4V by electron beam melting [D]. Sheffield: University of Sheffield, 2011
[21] Cheng B, Price S, Lydon J, et al. On process temperature in powder-bed electron beam additive manufacturing: Model development and validation [J]. J. Manuf. Sci. Eng., 2014, 136: 061018
doi: 10.1115/1.4028484
[22] Price S, Cheng B, Lydon J, et al. On process temperature in powder-bed electron beam additive manufacturing: Process parameter effects [J]. J. Manuf. Sci. Eng., 2014, 136: 061019
doi: 10.1115/1.4028485
[23] Attar H, Calin M, Zhang L C, et al. Manufacture by selective laser melting and mechanical behavior of commercially pure titanium [J]. Mater. Sci. Eng., 2014, A593: 170
[24] Liu Y J, Liu Z, Jiang Y, et al. Gradient in microstructure and mechanical property of selective laser melted AlSi10Mg [J]. J. Alloys Compd., 2018, 735: 1414
doi: 10.1016/j.jallcom.2017.11.020
[25] Krishna B V, Bose S, Bandyopadhyay A. Laser processing of net-shape NiTi shape memory alloy [J]. Metall. Mater. Trans., 2007, 38A: 1096
[26] Gong H J, Rafi K, Gu H F, et al. Influence of defects on mechanical properties of Ti-6Al-4 V components produced by selective laser melting and electron beam melting [J]. Mater. Des., 2015, 86: 545
doi: 10.1016/j.matdes.2015.07.147
[27] Li Y T. The study on defect formation in laser additive manufacturing titanium alloy [D]. Dalian: Dalian University of Technology, 2017
[27] (李永涛. 钛合金激光增材制造缺陷研究 [D]. 大连: 大连理工大学, 2017)
[1] 张雷雷, 陈晶阳, 汤鑫, 肖程波, 张明军, 杨卿. K439B铸造高温合金800℃长期时效组织与性能演变[J]. 金属学报, 2023, 59(9): 1253-1264.
[2] 卢楠楠, 郭以沫, 杨树林, 梁静静, 周亦胄, 孙晓峰, 李金国. 激光增材修复单晶高温合金的热裂纹形成机制[J]. 金属学报, 2023, 59(9): 1243-1252.
[3] 孙蓉蓉, 姚美意, 王皓瑜, 张文怀, 胡丽娟, 仇云龙, 林晓冬, 谢耀平, 杨健, 董建新, 成国光. Fe22Cr5Al3Mo-xY合金在模拟LOCA下的高温蒸汽氧化行为[J]. 金属学报, 2023, 59(7): 915-925.
[4] 吴东江, 刘德华, 张子傲, 张逸伦, 牛方勇, 马广义. 电弧增材制造2024铝合金的微观组织与力学性能[J]. 金属学报, 2023, 59(6): 767-776.
[5] 张东阳, 张钧, 李述军, 任德春, 马英杰, 杨锐. 热处理对选区激光熔化Ti55531合金多孔材料力学性能的影响[J]. 金属学报, 2023, 59(5): 647-656.
[6] 李殿中, 王培. 金属材料的组织定制[J]. 金属学报, 2023, 59(4): 447-456.
[7] 朱智浩, 陈志鹏, 刘田雨, 张爽, 董闯, 王清. 基于不同 α / β 团簇式比例的Ti-Al-V合金的铸态组织和力学性能[J]. 金属学报, 2023, 59(12): 1581-1589.
[8] 芮祥, 李艳芬, 张家榕, 王旗涛, 严伟, 单以银. 新型纳米复合强化9Cr-ODS钢的设计、组织与力学性能[J]. 金属学报, 2023, 59(12): 1590-1602.
[9] 彭立明, 邓庆琛, 吴玉娟, 付彭怀, 刘子翼, 武千业, 陈凯, 丁文江. 镁合金选区激光熔化增材制造技术研究现状与展望[J]. 金属学报, 2023, 59(1): 31-54.
[10] 葛进国, 卢照, 何思亮, 孙妍, 殷硕. 电弧熔丝增材制造2Cr13合金组织与性能各向异性行为[J]. 金属学报, 2023, 59(1): 157-168.
[11] 杨天野, 崔丽, 贺定勇, 黄晖. 选区激光熔化AlSi10Mg-Er-Zr合金微观组织及力学性能强化[J]. 金属学报, 2022, 58(9): 1108-1117.
[12] 李彦强, 赵九洲, 江鸿翔, 何杰. Pb-Al合金定向凝固组织形成过程[J]. 金属学报, 2022, 58(8): 1072-1082.
[13] 张鑫, 崔博, 孙斌, 赵旭, 张欣, 刘庆锁, 董治中. Y元素对Cu-Al-Ni高温形状记忆合金性能的影响[J]. 金属学报, 2022, 58(8): 1065-1071.
[14] 刘仁慈, 王鹏, 曹如心, 倪明杰, 刘冬, 崔玉友, 杨锐. 700℃热暴露对 β 凝固 γ-TiAl合金表面组织及形貌的影响[J]. 金属学报, 2022, 58(8): 1003-1012.
[15] 张家榕, 李艳芬, 王光全, 包飞洋, 芮祥, 石全强, 严伟, 单以银, 杨柯. 热处理对一种双峰晶粒结构超低碳9Cr-ODS钢显微组织与力学性能的影响[J]. 金属学报, 2022, 58(5): 623-636.