DISLOCATION CREEP IN SUPER–LIGHT α SOLID SOLUTION BASE Mg–6Li–3Zn ALLOY |
CAO Furong1; GUAN Renguo1; DING Hua1; LI Yinglong1; ZHOU Ge1;CUI Jianzhong2 |
1.College of Materials and Metallurgy; Northeastern University; Shenyang 110819
2.Key Lab of Materials Electromagnetic Process; Ministry of Education; Northeastern University; Shenyang 110819 |
|
Cite this article:
CAO Furong GUAN Renguo DING Hua LI Yinglong ZHOU Ge CUI Jianzhong. DISLOCATION CREEP IN SUPER–LIGHT α SOLID SOLUTION BASE Mg–6Li–3Zn ALLOY. Acta Metall Sin, 2010, 46(6): 715-722.
|
Abstract Mg–6Li–3Zn alloy was prepared by Jackson’s melting and casting method and the sheets of 1.2 mm in thickness processed by hot rolling at 573 K and cold rolling with a total reduction of more than 92% were obtained. The high–temperature mechanical behavior at temperatures ranging
from 423 to 673 K and initial strain rates ranging from 1.67×10−3 to 5×10−2 s−1 were investigated. The microstructure evolution, such as grains, subgrains, dislocations, cavities and fracture morphology, were investigated by OM, TEM and SEM. Yavari–Langdon model describing the transition between dislocatoviscous glide and dislocation climb was used to construct a new dislocatiocreep mechanism map which consists of Cottrell’s solute atmosphere breakaway dislocation climb regime, dislocation viscous glide regime and Cottrell’s solute atmosphere incorporated dislocation climb regime. A new cavity growth map considering cavity coalescence was obtained according to the cavity growth models. The maximum elongation to failure of 300% was demonstrated at 623 K and an initial strain rate of 1.67×10−3 s−1. Significant dynamic recrystallization occurred in band–like structure at 573 K and an initial strain rate of 1.67×10−3 s−1, the subgrain contour was ambiguous and dislocation distribution was relatively uniform. Fracture mode of the alloy at 573—623 K and an initial strain rate of 1.67×10−3 s−1 is ductile fracture. It is shown by the dislocation creep mechanism map that the high–temperature deformation mechaism in Mg–6Li–3Zn alloy sheet with bad–like structure at 573 K and an initial strain rate of .67×10−3 s−1 is dislocation viscous glide cotrolled by lattice diffusion, the stress exponent is 3 (strain rate sesitivity exponent 0.33) and deformation activation energy is 134.8 kJ/mol, which is the samas the lattice diffusion activation energy of Mg. The cavity growth mechanism of the alloy at 573 K and iitial strain rate of 1.67×10−3 s−1 is plasticity controlled cavity growth.
|
Received: 07 September 2009
|
Fund: Supported by National Natural Science Foundation of China (Nos.50774023 and 50974038), National High Technology Research and Development Program of China (No.2007AA03Z111) and China Central University Basic Research Transaction Expenses (No.090502003) |
[1] Counts W A, Friak M, Raabe D, Neugebauer J. Acta Mater, 2009; 57: 69
[2] Kim W J, Kim M J, Wang J Y. Mater Sci Eng, 2009; A516: 17
[3] Cao F R, Lei F, Cui J Z, Wen J L. Acta Metall Sin, 1999; 35: 770
(曹富荣, 雷方, 崔建忠, 温景林. 金属学报, 1999; 35: 770)
[4] Nayeb–Hashemi A A, Clark J B, Pelton A D. Bull Alloy Phase Diagram, 1984; 5: 365
[5] Raynor G V. The Physical Metallurgy of Magnesium and Its Alloys. London: Pergamon Press, 1959: 25
[6] Kassner M E, Perez–Prado M T. Prog Mater Sci, 2000; 45: 1
[7] Yavari P, Langdon T G. Acta Metall, 1982; 30: 2181
[8] Somekawa H, Hirai K, Watanabe H, Takigawa Y, Higashi K. Mater Sci Eng, 2005; A407: 53
[9] Li Y, Langdon T G. Acta Mater, 1998; 46: 1143
[10] Weinberg A F, Levinson D W, Rostoker W. Trans ASM, 1956; 48: 855
[11] Cao F R, Ding H, Li Y L, Zhou G, Cui J Z. Mater Sci Eng, 2010, A527: 2335
[12] Sherby O D, Wadsworth J. In: Krauss G ed., Deformation, Processing and Structure. Metals Park, Ohio: ASM, 1982: 355
[13] Hirai K, Somekawa H, Takigawa Y, Higashi K. Scr Mater, 2007; 56: 237
[14] King H W. J Mater Sci, 1966; 1: 79
[15] Murr L E. Interfacial Phenomena in Metals and Alloys. Mass: Addison Wesley, 1975: 55
[16] Koster W. Z Metallk, 1948; 39: 1
[17] Friedel J. Dislocations. Oxford: Pergamon Press, 1964: 202
[18] Wang J S, Nix W D. Acta Metall, 1986; 34: 545
[19] Fuentes–Samaniego R, Nix W D. Scr Metall, 1981; 15: 15
[20] Brown A W, Ashby M F. Acta Metall, 1980; 28: 1085
[21] Wolfenstine J, Gonzalez–Docel G, Sherby O D. J Mater Res, 1990; 5: 1359
[22] Ruano O A, Wadsworth J, Sherby O D. J Mater Sci, 1985; 20: 3735
[23] Pilling J, Ridley N. Superplasticity in Crystalline Solids. London: The Institute of Metals, 1989: 118
[24] Cao F R. PhD Thesis, Northeastern University, Shenyang, 1999
(曹富荣. 东北大学博士学位论文, 沈阳, 1999)
[25] Stowell M J, Livesey D W, Ridley N. Acta Metall, 1984; 32: 35
[26] Mukherjee A K. Mater Sci Eng, 1971; 8: 83
[27] Taleff E M, Ruano O A, Wolfenstine J, Sherby O D. J Mater Res, 1992; 7: 2131 |
No Suggested Reading articles found! |
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
|
Shared |
|
|
|
|
|
Discussed |
|
|
|
|