Abstract The effect of the contents of
ZrO2(3Y) and ZrO2(2Y) on the mechanical properties of the
Al2O3/ZrO3(Y2O3)
composites prepared by vacuum sintering has been studied.
The change of m--ZrO2 and
t-ZrO2 contents before and after fracture
was detarmined by X-ray diffraction phase analysis,
which is related to the toughening mechanism.
When the content of ZrO2 is 15% (volume frection), the bending
strength and fracture toughness of Al2O3/ZrO2(2Y)
composite are 738 MPa and 6.7 MPa.m1/2, respectively, while
those of the Al2O3/ZrO2(3Y) composite are 825 MPa and 7.8
MPa.m1/2, respectively. The difference in mechanical
properties is due to the operation of different toughening
mechanisms.
[1] Munro R G. J Am Ceram Soc, 1997; 80: 1919 [2] Rao P G,Iwasa M,Kondih I. J Mater Sci Lett, 2000; 19:543 [3] Garvie R C, Hannink R H, Pascoe R T. Nature, 1975; 258:703 [4] Claussen N. J Am Ceram Soc, 1976; 59: 49 [5] Shin D W, Orr K K, Schubert H. J Am Ceram Soc,1990; 73: 1181 [6] Mullot J, Lecompte J P, Montanaro L, Negro A. J Euro Ceram Soc, 1993; 11: 309 [7] Kishino J, Nishiyama A, Sakuma T. J Mater Sci, 1996;31: 4991 [8] Li J F, Watanabe R. J Mater Sci, 1999; 32: 1149 [9] Chevalier J,Cales B, Drouin J M. J Am Ceram Soc, 1999;82: 2150 [10] Ohhmichi N, Kamioka K, Uede K, Matsui K, Ohgai M. JCeram Soc Jpn, 1999; 107(2): 128 [11] Zhu W Z, Zhang X B. Scr Mater,1999; 40: 1229 [12] Lange F F, Dunlop G L, Davis B I. J Am Ceram Soc,1986; 69(3): 237 [13] Tsukuma K. Am Ceram Soc Bull, 1986; 65: 1386 [14] Li J G, Sun X D. Acta Mater, 2000; 48: 3103 [15] Lin J D, Duh J G. J Mater Sci, 1997; 32: 4901 [16] Lange F F. J Mater Sci, 1982; 17: 247 [17] Becher P F. J Am Ceram Soc, 1991; 74: 255 [18] Shi J L, Li B S, Lu Z L, Huang X X, Yan D S. Chin JMater Res, 1996; 10(1): 51(施剑林,李包顺,陆正兰,黄校先,严东生.材料研究学报,1996;10(1):51) [19] Lange F F. J Mater Sci, 1982; 17: 235 [20] Clussen N. J Am Ceram Soc, 1987; 61: 85 [21] Lange F F. J Mater Sci, 1982; 17: 225 [22] Evans A G. J Am Ceram Soc, 1990; 73: 187.