Please wait a minute...
金属学报  2019, Vol. 55 Issue (10): 1319-1328    DOI: 10.11900/0412.1961.2018.00523
  本期目录 | 过刊浏览 |
热压烧结温度对SiC/Al-Zn-Mg-Cu复合材料微观结构与力学性能的影响
马国楠1,2,王东1(),刘振宇1,毕胜1,2,昝宇宁1,2,肖伯律1,马宗义1
1. 中国科学院金属研究所沈阳材料科学国家研究中心 沈阳 110016
2. 中国科学技术大学材料科学与工程学院 沈阳 110016
Effect of Hot Pressing Temperature on Microstructure and Tensile Properties of SiC/Al-Zn-Mg-Cu Composites
MA Guonan1,2,WANG Dong1(),LIU Zhenyu1,BI Sheng1,2,ZAN Yuning1,2,XIAO Bolv1,MA Zongyi1
1. Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
2. School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
引用本文:

马国楠, 王东, 刘振宇, 毕胜, 昝宇宁, 肖伯律, 马宗义. 热压烧结温度对SiC/Al-Zn-Mg-Cu复合材料微观结构与力学性能的影响[J]. 金属学报, 2019, 55(10): 1319-1328.
Guonan MA, Dong WANG, Zhenyu LIU, Sheng BI, Yuning ZAN, Bolv XIAO, Zongyi MA. Effect of Hot Pressing Temperature on Microstructure and Tensile Properties of SiC/Al-Zn-Mg-Cu Composites[J]. Acta Metall Sin, 2019, 55(10): 1319-1328.

全文: PDF(20713 KB)   HTML
摘要: 

利用粉末冶金法制备了含15%SiC (体积分数)的SiC/Al-7.5Zn-2.8Mg-1.7Cu (质量分数,%)复合材料,采用TEM、EPMA和拉伸实验等分析测试手段,研究了热压烧结温度(500~560 ℃)对复合材料微观组织和力学性能的影响。结果表明,所选热压温度下均可制备致密无孔洞的复合材料坯锭。热压温度为500和520 ℃时,SiC/Al界面反应程度较轻,挤压棒材经T6热处理后,Zn元素均匀分布于基体中,但存在的少量富Mg微米级难溶相使复合材料的力学性能产生较大波动。当热压温度升高到540 ℃时,富Mg难溶相尺寸明显减小,元素分布变得更均匀,复合材料力学性能稳定性明显提升。当热压温度继续升高到560 ℃时,Mg元素开始向SiC颗粒周围偏聚,界面反应更加严重,而且降低了基体中MgZn2的体积分数,使复合材料抗拉强度明显下降。对560 ℃热压的复合材料进行高角度环形暗场像和EDS分析,发现SiC/Al界面同时存在含Mg氧化物和粗大的MgZn2沉淀相。

关键词 : 粉末冶金,  金属基复合材料,  界面,  析出相    
Abstract:

Particulate reinforced aluminum matrix composites have been widely used in industrial fields. In general, high strength aluminium alloys, such as 2024Al are employed to produce stronger composites. However, the composites with high strength Al-Zn-Mg-Cu alloys as the matrices are paid relative attentions. Therefore, the corresponding optimization for fabrication parameters has not been well understood. In the present work, SiC particles with volume fraction of 15% reinforced Al-7.5Zn-2.8Mg-1.7Cu (mass fraction, %) composites were fabricated using powder metallurgy (PM) technique at hot pressing temperatures of 500, 520, 540 and 560 ℃. TEM, EPMA and tensile test were used to study the effect of hot pressing temperature on the microstructure and tensile properties of SiC/Al-Zn-Mg-Cu composites. The measured densities indicated that all the composites were completely condensed, no pores were observed. Undissolved phase containing Mg and Cu segregated in matrix of the composites hot pressed at 500 and 520 ℃, resulting in instable tensile properties. With increasing hot pressing temperature to 540 ℃, Mg and Cu were uniformly distributed in the composites which exhibited the stable tensile properties. With further increasing temperature to 560 ℃, Mg segregated around SiC particles due to interface reaction. In this case, the content of MgZn2 phase was decreased, resulting in the reduction of tensile strength. HAADF-STEM and EDS analyses showed that the interface compounds were oxide of Mg and coarse MgZn2 phase.

Key words: powder metallurgy    metal matrix composite    interface    precipitate
收稿日期: 2018-11-20     
ZTFLH:  TG146.2  
基金资助:国家重点研发计划项目(52017YFB0703104);国家自然科学基金项目(51771193);国家自然科学基金项目(U1508216)
作者简介: 马国楠,男,1992年生,博士生
Hot pressing temperature / ℃Measured density / (g·cm-3)Relative density / %
5002.87799.93
5202.87899.96
5402.879100.00
5602.881100.01
表1  不同热压温度制备热压态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料的测量密度和致密度
图1  不同热压温度制备的SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料挤压棒材显微组织的OM像
图2  SiC颗粒分布的均匀性
图3  不同热压温度制备的SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料的XRD谱
图4  500 ℃热压烧结T6态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料的SE-SEM像和元素分布图
图5  不同热压温度制备T6态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料的SE-SEM像和元素分布图
图6  不同热压温度制备T6态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料的界面TEM像和HAADF-STEM像
图7  560 ℃下热压的T6态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料界面产物的TEM像和元素分布图

Hot pressing temperature

℃

Tensile strength

MPa

Yield strength

MPa

Elongation

%

500679±13645±192.8±0.6
520675±8637±103.0±0.4
540671±6632±63.2±0.6
560658±10620±103.4±0.4
表2  不同热压温度制备T6态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料的拉伸性能
图8  不同热压温度制备T6态SiC/Al-7.5Zn-2.8Mg-1.7Cu复合材料试样断口形貌的SEM像
[1] Song J Y, Guo Q, Ouyang Q B, et al. Influence of interfaces on the mechanical behavior of SiC particulate-reinforced Al-Zn-Mg-Cu composites [J]. Mater. Sci. Eng., 2015, A644: 79
[2] Xiao B L, Huang Z Z, Ma K, et al. Research on hot deformation behaviors of discontinuously reinforced aluminum composites [J]. Acta Metall. Sin., 2019, 55: 59
[2] (肖伯律, 黄治治, 马 凯等. 非连续增强铝基复合材料的热变形行为研究进展 [J]. 金属学报, 2019, 55: 59)
[3] Li B, Luo B H, He K J ,et al. Effect of aging on interface characteristics of Al-Mg-Si/SiC composites [J]. J. Alloys Compd., 2015, 649: 495
[4] Monazzah A H, Pouraliakbar H, Bagheri R ,et al. Al-Mg-Si/SiC laminated composites: Fabrication, architectural characteristics, toughness, damage tolerance, fracture mechanisms [J]. Composites, 2017, 125B: 49
[5] Wang Z G, Li C P, Wang H Y, et al. Aging behavior of Nano-SiC/2014Al composite fabricated by powder metallurgy and hot extrusion techniques [J]. J. Mater. Sci. Technol., 2016, 32: 1008
[6] Jin P, Xiao B L, Wang Q Z ,et al. Effect of solution temperature on aging behavior and properties of SiCp/Al-Cu-Mg composites [J]. Mater. Sci. Eng., 2011, A528: 1504
[7] Kalkanl? A, Y?lmaz S. Synthesis and characterization of aluminum alloy 7075 reinforced with silicon carbide particulates [J]. Mater. Des., 2008, 29: 775
[8] Sharma M M, Amateau M F, Eden T J. Aging response of Al-Zn-Mg-Cu spray formed alloys and their metal matrix composites [J]. Mater. Sci. Eng., 2006, A424: 87
[9] Min K H, Lee B H, Chang S Y ,et al. Mechanical properties of sintered 7xxx series Al/SiCp composites [J]. Mater. Lett., 2007, 61: 2544
[10] Dasgupta R, Meenai H. SiC particulate dispersed composites of an Al-Zn-Mg-Cu alloy: Property comparison with parent alloy [J]. Mater. Charact., 2005, 54: 438
[11] Kumar N V R, Dwarakadasa E S. Effect of matrix strength on the mechanical properties of Al-Zn-Mg/SiCp composites [J]. Composites, 2000, 31A: 1139
[12] Manoharan M, Lewandowski J J. Effect of reinforcement size and matrix microstructure on the fracture properties of an aluminum metal matrix composite [J]. Mater. Sci. Eng., 1992, A150: 179
[13] Evans R D, Boyd J D. Near-interface microstructure in a SiC/Al composite [J]. Scr. Mater., 2003, 49: 59
[14] Hong S H, Chung K H. Effects of vacuum hot pressing parameters on the tensile properties and microstructures of SiC-2124 A1 composites [J]. Mater. Sci. Eng., 1995, A194: 165
[15] Cheng N P, Zeng S M, Wang S B ,et al. Effects of forming temperature on properties of SiCP/Al composite [J]. Hot Work. Technol., 2007, 32(2): 13
[15] (程南璞, 曾苏民, 王水兵等. 成形温度对SiCP/Al复合材料性能的影响 [J]. 热加工工艺, 2007, 32(2): 13)
[16] Li Y Z, Wang Q Z, Wang W G, et al. Interfacial reaction mechanism between matrix and reinforcement in B4C/6061Al composites [J]. Mater. Chem. Phys., 2015, 154: 107
[17] Ma W C, Gu J L, Zhang Y ,et al. Effect of SiC particles on ageing behaviour of SiCp/7075 composites [J]. J. Mater. Sci. Lett., 1997, 16: 1867
[18] Lee K B, Kwon H. Strength of Al-Zn-Mg-Cu matrix composite reinforced with SiC particles [J]. Metall. Mater. Trans., 2002, 33A: 455
[19] Thébaud F, Hervé E, Da Silva R ,et al. The effect of the interfacial strength on the overall mechanical properties of particle reinforced metal matrix composites [A]. 2nd International Conference on Interfacial Phenomena in Composite Materials [C]. Louvain, Belgium, 1991: 179
[20] Man C F, Mummery P M, Derby B, et al. The influence of magnesium segregation on the fracture of silicon carbide particle-reinforced aluminium metal matrix composites [A]. 2nd International Conference on Interfacial Phenomena in Composite Materials [C]. Louvain, Belgium, 1991: 175
[21] Liu Z Y, Wang Q Z, Xiao B L ,et al. Effects of double extrusion on the microstructure and tensile property of the PM processed SiCp/2009Al composites [J]. Acta Metall. Sin., 2010, 46: 1121
[21] (刘振宇, 王全兆, 肖伯律等. 二次挤压对SiCp/2009Al复合材料微观结构和力学性能的影响 [J]. 金属学报, 2010, 46: 1121)
[22] Ogel B, Gurbuz R. Microstructural characterization and tensile properties of hot pressed Al-SiC composites prepared from pure Al and Cu powders [J]. Mater. Sci. Eng., 2001, A301: 213
[23] Zhou J, Duszczyk J. Liquid phase sintering of an AA2014-based composite prepared from an elemental powder mixture [J]. J. Mater. Sci., 1999, 34: 545
[24] Zhang Q, Wang Q Z, Xiao B L, et al. Phases and elemental distributions in SiCp/Al-Cu-Mg composite fabricated by powder metallurgy [J]. Acta Metall. Sin., 2012, 48: 135
[24] (张 琪, 王全兆, 肖伯律等. 粉末冶金制备SiCp/2009Al复合材料的相组成和元素分布 [J]. 金属学报, 2012, 48: 135)
[25] Li B, Pan Q L, Chen C P ,et al. Effects of solution treatment on microstructural and mechanical properties of Al-Zn-Mg alloy by microalloying with Sc and Zr [J]. J. Alloys Compd., 2016, 664: 553
[26] Wang D, Xiao B L, Wang Q Z ,et al. Evolution of the microstructure and strength in the nugget zone of friction stir welded SiCp/Al-Cu-Mg composite [J]. J. Mater. Sci. Technol., 2014, 30: 54
[27] Kiourtsidis G E, Skolianos S M, Litsardakis G A. Aging response of aluminium alloy 2024/silicon carbide particles (SiCp) composites [J]. Mater. Sci. Eng., 2004, A382: 351
[28] Ure?a A, Mart??nez E E, Rodrigo P ,et al. Oxidation treatments for SiC particles used as reinforcement in aluminium matrix composites [J]. Compos. Sci. Technol., 2004, 64: 1843
[29] McLeod A D, Gabryel C M. Kinetics of the growth of spinel, MgAl2O4, on alumina particulate in aluminum alloys containing magnesium [J]. Metall. Mater. Trans., 1992, 23A: 1279
[30] Strangwood M, Hippsley C A, Lewandowski J J. Segregation to SiC/Al interfaces in Al based metal matrix composites [J]. Scr. Metall. Mater., 1990, 24: 1483
[31] Shi Z L, Ochiai S, Hojo M ,et al. The oxidation of SiC particles and its interfacial characteristics in Al-matrix composite [J]. J. Mater. Sci., 2001, 36: 2441
[32] Jin P, Xiao B L, Wang Q Z ,et al. Effect of hot pressing temperature on microstructure and mechanical properties of SiC particle reinforced aluminum matrix composites [J]. Acta Metall. Sin., 2011, 47: 298
[32] (金 鹏, 肖伯律, 王全兆等. 热压烧结温度对SiC颗粒增强铝基复合材料微观组织及力学性能的影响 [J]. 金属学报, 2011, 47: 298)
[33] Shin K, Chung D S, Lee S. The effect of consolidation temperature on microstructure and mechanical properties in powder metallurgy-processed 2XXX aluminum alloy composites reinforced with SiC particulates [J]. Metall. Mater. Trans., 1997, 28
[1] 宫声凯, 刘原, 耿粒伦, 茹毅, 赵文月, 裴延玲, 李树索. 涂层/高温合金界面行为及调控研究进展[J]. 金属学报, 2023, 59(9): 1097-1108.
[2] 王宗谱, 王卫国, Rohrer Gregory S, 陈松, 洪丽华, 林燕, 冯小铮, 任帅, 周邦新. 不同温度轧制Al-Zn-Mg-Cu合金再结晶后的{111}/{111}近奇异晶界[J]. 金属学报, 2023, 59(7): 947-960.
[3] 梁凯, 姚志浩, 谢锡善, 姚凯俊, 董建新. 新型耐热合金SP2215组织与性能的关联性[J]. 金属学报, 2023, 59(6): 797-811.
[4] 王福容, 张永梅, 柏国宁, 郭庆伟, 赵宇宏. Al掺杂Mg/Mg2Sn合金界面的第一性原理计算[J]. 金属学报, 2023, 59(6): 812-820.
[5] 徐磊, 田晓生, 吴杰, 卢正冠, 杨锐. 热等静压成形Inconel 718粉末合金的显微组织和力学性能[J]. 金属学报, 2023, 59(5): 693-702.
[6] 李谦, 孙璇, 罗群, 刘斌, 吴成章, 潘复生. 镁基材料中储氢相及其界面与储氢性能的调控[J]. 金属学报, 2023, 59(3): 349-370.
[7] 夏大海, 计元元, 毛英畅, 邓成满, 祝钰, 胡文彬. 2024铝合金在模拟动态海水/大气界面环境中的局部腐蚀机制[J]. 金属学报, 2023, 59(2): 297-308.
[8] 朱云鹏, 覃嘉宇, 王金辉, 马鸿斌, 金培鹏, 李培杰. 机械球磨结合粉末冶金制备AZ61超细晶镁合金的组织与性能[J]. 金属学报, 2023, 59(2): 257-266.
[9] 陈凯旋, 李宗烜, 王自东, Demange Gilles, 陈晓华, 张佳伟, 吴雪华, Zapolsky Helena. Cu-2.0Fe合金等温处理过程中富Fe析出相的形态演变[J]. 金属学报, 2023, 59(12): 1665-1674.
[10] 马国楠, 朱士泽, 王东, 肖伯律, 马宗义. SiC颗粒增强Al-Zn-Mg-Cu复合材料的时效行为和力学性能[J]. 金属学报, 2023, 59(12): 1655-1664.
[11] 芮祥, 李艳芬, 张家榕, 王旗涛, 严伟, 单以银. 新型纳米复合强化9Cr-ODS钢的设计、组织与力学性能[J]. 金属学报, 2023, 59(12): 1590-1602.
[12] 周小宾, 赵占山, 汪万行, 徐建国, 岳强. 渣-金界面气泡夹带行为数值物理模拟[J]. 金属学报, 2023, 59(11): 1523-1532.
[13] 沈莹莹, 张国兴, 贾清, 王玉敏, 崔玉友, 杨锐. SiCf/TiAl复合材料界面反应及热稳定性[J]. 金属学报, 2022, 58(9): 1150-1158.
[14] 李小琳, 刘林锡, 李雅婷, 杨佳伟, 邓想涛, 王海丰. 单一 MX 型析出相强化马氏体耐热钢力学性能及蠕变行为[J]. 金属学报, 2022, 58(9): 1199-1207.
[15] 宋庆忠, 潜坤, 舒磊, 陈波, 马颖澈, 刘奎. 镍基高温合金K417G与氧化物耐火材料的界面反应[J]. 金属学报, 2022, 58(7): 868-882.