| 流动海水中多重应力耦合作用下B10 Cu-Ni合金的微观结构演变与动态失效机制 |
李瑞雪1, 周晨曦1, 杨慧敏1, 雍兴跃2( ), 刘景军1( ) |
1 北京化工大学 材料科学与工程学院 北京 100029 2 北京化工大学 化学工程学院 北京 100029 |
|
| Microstructural Evolution and Dynamic Failure Mechanism of B10 Cu-Ni Alloy Under Multiple Stress Coupling in Flowing Seawater |
LI Ruixue1, ZHOU Chenxi1, YANG Huimin1, YONG Xingyue2( ), LIU Jingjun1( ) |
1 School of Materials Science and Engineering, Beijing University of Chemical Technology, Beijing 100029, China 2 School of Chemical Engineering, Beijing University of Chemical Technology, Beijing 100029, China |
引用本文:
李瑞雪, 周晨曦, 杨慧敏, 雍兴跃, 刘景军. 流动海水中多重应力耦合作用下B10 Cu-Ni合金的微观结构演变与动态失效机制[J]. 金属学报, 2026, 62(7): 1273-1287.
Ruixue LI,
Chenxi ZHOU,
Huimin YANG,
Xingyue YONG,
Jingjun LIU.
Microstructural Evolution and Dynamic Failure Mechanism of B10 Cu-Ni Alloy Under Multiple Stress Coupling in Flowing Seawater[J]. Acta Metall Sin, 2026, 62(7): 1273-1287.
| [1] |
Lin L Y, Liu S F, Liu Z C, et al. Surface and interface characteristics of Cu-Ni alloy corroded in seawater [J]. Corros. Sci. Prot. Technol., 1999, 11(1): 37
|
| [1] |
林乐耘, 刘少峰, 刘增才 等. 铜镍合金海水腐蚀的表面与界面特征研究 [J]. 腐蚀科学与防护技术, 1999, 11(1): 37
|
| [2] |
Xia Q Q, Zhu T. Analysis and thinking of B10 material standard of ship sea pipeline [J]. Ship Stand. Eng., 2018, 51(4): 15
|
| [2] |
夏齐强, 朱 韬. 舰船海水管路B10材料标准分析与思考 [J]. 船舶标准化工程师, 2018, 51(4): 15
|
| [3] |
Luo X, Xin X, Li Y, et al. Progress on corrosion and repair technology of marine seawater pipe [J]. China Elastom., 2022, 32(1): 80
|
| [3] |
罗 旭, 辛 颉, 李 瑜 等. 船舶海水管路腐蚀及修复技术研究进展 [J]. 弹性体, 2022, 32(1): 80
|
| [4] |
Zhang Z Q, Guo Z L, Lei Z F. Applications of copper alloy in shipbuilding [J]. Dev. Appl. Mater., 2006, 21(5): 43
|
| [4] |
张智强, 郭泽亮, 雷竹芳. 铜合金在舰船上的应用 [J]. 材料开发与应用, 2006, 21(5): 43
|
| [5] |
Tian F, Bai X Q, He X Y, et al. Research progress on microbiological induced corrosion of metallic materials under ocean environment [J]. Surf. Technol., 2018, 47(8): 182
|
| [5] |
田 丰, 白秀琴, 贺小燕 等. 海洋环境下金属材料微生物腐蚀研究进展 [J]. 表面技术, 2018, 47(8): 182
|
| [6] |
Stack M M, Corlett N, Turgoose S. Some thoughts on modelling the effects of oxygen and particle concentration on the erosion-corrosion of steels in aqueous slurries [J]. Wear, 2003, 255: 225
doi: 10.1016/S0043-1648(03)00205-9
|
| [7] |
Xu Y. Numerical simulation study on erosion-corrosion induced by liquid-solid two-phase flow [D]. Beijing: Beijing University of Chemical Technology, 2001
|
| [7] |
徐 姚. 液固两相流冲刷腐蚀数值模拟研究 [D]. 北京: 北京化工大学, 2001
|
| [8] |
Leon A, Levy G K, Ron T, et al. The effect of strain rate on stress corrosion performance of Ti6Al4V alloy produced by additive manufacturing process [J]. J. Mater. Res. Technol., 2020, 9: 4097
doi: 10.1016/j.jmrt.2020.02.035
|
| [9] |
Ren P W. Study of tribocorrosion of three different corrosion reisistance materials under deep-sea high pressure [D]. Beijing: University of Science and Technology Beijing, 2022
|
| [9] |
任鹏伟. 三类不同耐蚀性材料在深海高压下的磨蚀研究 [D]. 北京: 北京科技大学, 2022
|
| [10] |
Liu R, Xie Y S, Jin Y, et al. Stress corrosion cracking of the titanium alloys under hydrostatic pressure resulting from the degradation of passive films [J]. Acta Mater., 2023, 252: 118946
doi: 10.1016/j.actamat.2023.118946
|
| [11] |
Dai J W, Zhang X G, Zhang L, et al. In vitro corrosion behavior of biodegradable WE43 alloy under various physiological flow velocities [J]. J. Mater. Sci., 2024, 59: 7854
doi: 10.1007/s10853-024-09617-1
|
| [12] |
Du J, Wang H R, Du M, et al. Electrochemical corrosion behavior of 90/10 Cu-Ni alloy in flowing seawater [J]. Corros. Sci. Prot. Technol., 2008, 20: 12
|
| [12] |
杜 娟, 王洪仁, 杜 敏 等. B10铜镍合金流动海水冲刷腐蚀电化学行为 [J]. 腐蚀科学与防护技术, 2008, 20: 12
|
| [13] |
Li X M, Zhang Y M, Guo X H, et al. Erosion corrosion behavior of copper-nickel alloy pipe in flowing seawater [J]. J. Henan Univ. Sci. Technol. (Nat. Sci.), 2017, 38(3): 10
|
| [13] |
李晓孟, 张彦敏, 国秀花 等. 流动海水中铜镍合金管材的冲刷腐蚀行为 [J]. 河南科技大学学报(自然科学版), 2017, 38(3): 10
|
| [14] |
Islam M A, Farhat Z N, Ahmed E M, et al. Erosion enhanced corrosion and corrosion enhanced erosion of API X-70 pipeline steel [J]. Wear, 2013, 302: 1592
doi: 10.1016/j.wear.2013.01.041
|
| [15] |
Ren P W. Study on erosion-corrosion behavior of X70 steel in simulated deep sea environment [D]. Nanning: Guangxi University, 2023
|
| [15] |
任鹏炜. X70钢在模拟深海环境下的冲刷腐蚀行为研究 [D]. 南宁: 广西大学, 2023
|
| [16] |
Yuan S J, Pehkonen S O. Surface characterization and corrosion behavior of 70/30 Cu-Ni alloy in pristine and sulfide-containing simulated seawater [J]. Corros. Sci., 2007, 49: 1276
doi: 10.1016/j.corsci.2006.07.003
|
| [17] |
Zhang R W. Effect of iron and manganese on corrosion resistance of B10 copper-nickel alloy and its mechanism [D]. Ganzhou: Jiangxi University of Science and Technology, 2019
|
| [17] |
张荣伟. 铁、锰对B10白铜合金耐蚀性能的影响及机理研究 [D]. 赣州: 江西理工大学, 2019
|
| [18] |
Wang Y Q, Shao Y W, Meng G Z, et al. Study on passivating treatment of Cu-Ni alloy in compound passivant containing benzotriazole [J]. Acta Metall. Sin., 2012, 48: 744
doi: 10.3724/SP.J.1037.2012.00032
|
| [18] |
王艳秋, 邵亚薇, 孟国哲 等. Cu-Ni合金BTA复配体系钝化处理工艺研究 [J]. 金属学报, 2012, 48: 744
doi: 10.3724/SP.J.1037.2012.00032
|
| [19] |
Aigbodion V S, Ozor P O, Eke M N, et al. Explicit microstructure, corrosion, and stress analysis of value-added Al-3.7%Cu-1.4%Mg/1.5% rice husk ash nanoparticles for pump impeller application [J]. Chem. Data Collect., 2021, 33: 100675
doi: 10.1016/j.cdc.2021.100675
|
| [20] |
Yan Y J, Huang J, Pan L, et al. A comparative study of methods for calculating the dislocation density in GaN-on-Si epitaxial wafers [J]. Micromachines, 2024, 15: 954
doi: 10.3390/mi15080954
|
| [21] |
Zak A K, Majid W H A, Abrishami M E, et al. X-ray analysis of ZnO nanoparticles by Williamson-Hall and size-strain plot methods [J]. Solid State Sci., 2011, 13: 251
doi: 10.1016/j.solidstatesciences.2010.11.024
|
| [22] |
Delley B. An all-electron numerical method for solving the local density functional for polyatomic molecules [J]. J. Chem. Phys., 1990, 92: 508
|
| [23] |
Chen Z M, Jin C, Ji X Y, et al. Atomistic understanding of Pt-based medium entropy alloys for oxygen reduction electrocatalysis based on first principles [J]. Int. J. Hydrogen Energy, 2023, 48: 160
doi: 10.1016/j.ijhydene.2022.09.247
|
| [24] |
Baker M D, Baker A D, Belanger J, et al. Linear relationship between weighted-average madelung constants and density functional theory energies for MgO nanotubes [J]. J. Phys. Chem., 2012, 116C: 25588
|
| [25] |
Luo Z L, Gao W, Jiang Q. Determinants of vacancy formation and migration in high-entropy alloys [J]. Sci. Adv., 2025, 11: eadr4697
doi: 10.1126/sciadv.adr4697
|
| [26] |
Schultz P A. First-principles calculations of metal surfaces. I. Slab-consistent bulk reference for convergent surface properties [J]. Phys. Rev., 2021, 103B: 195426
|
| [27] |
Canneaux S, Bohr F, Henon E. KiSThelP: A program to predict thermodynamic properties and rate constants from quantum chemistry results [J]. J. Comput. Chem., 2014, 35: 82
pmid: 24190715
|
| [28] |
Halgren T A, Lipscomb W N. The synchronous-transit method for determining reaction pathways and locating molecular transition states [J]. Chem. Phys. Lett., 1977, 49: 225
doi: 10.1016/0009-2614(77)80574-5
|
| [29] |
Zhang W Q, Han S J, Zhang D W, et al. Variations in dissolved oxygen and aquatic biological responses in China’s coastal seas [J]. Environ. Res., 2023, 223: 115418
doi: 10.1016/j.envres.2023.115418
|
| [30] |
Jarvis B M, Greene R M, Wan Y S, et al. Contiguous low oxygen waters between the continental shelf hypoxia zone and nearshore coastal waters of Louisiana, USA: Interpreting 30 years of profiling data and three-dimensional ecosystem modeling [J]. Environ. Sci. Technol., 2021, 55: 4709
doi: 10.1021/acs.est.0c05973
|
| [31] |
Rouf M A, Islam M J, Roknuzzaman M, et al. Vertical profile of dissolved oxygen and associated water variables in the Pasur-Rupsha estuary of Bangladesh [J]. Heliyon, 2022, 8: e10935
doi: 10.1016/j.heliyon.2022.e10935
|
| [32] |
Li B, Zhang L, Yan T Y, et al. Effects of heat treatment processes and W wire properties on residual stress in W wire reinforced Zr-based metallic glass composites [J]. Acta Metall. Sin., 2024, 60: 1055
doi: 10.11900/0412.1961.2024.00066
|
| [32] |
李 彪, 张 龙, 颜廷毅 等. 热处理工艺和W丝特性对W丝增强锆基非晶复合材料残余应力的影响 [J]. 金属学报, 2024, 60: 1055
|
| [33] |
Chakrahari K K, Liao J H, Kahlal S, et al. [Cu13{S2CN n Bu2}6-(acetylide)4]+: A two-electron superatom [J]. Angew. Chem. Int. Ed., 2016, 55: 14704
doi: 10.1002/anie.v55.47
|
| [34] |
Zhang J M, Ma F, Xu K W. Calculation of the surface energy of FCC metals with modified embedded-atom method [J]. Appl. Surf. Sci., 2004, 229: 34
doi: 10.1016/j.apsusc.2003.09.050
|
| [35] |
Han Y, Lai K C, Lii-Rosales A, et al. Surface energies, adhesion energies, and exfoliation energies relevant to copper-graphene and copper-graphite systems [J]. Surf. Sci., 2019, 685: 48
doi: 10.1016/j.susc.2019.01.009
|
| [36] |
Deng J, Wang C, Guan G Z, et al. The deformations of carbon nanotubes under cutting [J]. ACS Nano, 2017, 11: 8464
doi: 10.1021/acsnano.7b04130
pmid: 28767215
|
| [37] |
Davis H L, Faulkner J S, Joy H W. Calculation of the band structure for copper as a function of lattice spacing [J]. Phys. Rev., 1968, 167: 601
doi: 10.1103/PhysRev.167.601
|
| [38] |
Zhu J, Li Z, Yang S T, et al. Characterization of strain field distribution in carbon fiber reinforced resin matrix composites using electron beam moiré and geometric phase analysis [J]. Opt. Lasers Eng., 2023, 163: 107457
doi: 10.1016/j.optlaseng.2022.107457
|
| [39] |
Meng Z K, Meng Z C, Gao C Y, et al. Molecular dynamics simulation of creep mechanism in nanocrystalline α-zirconium under various conditions [J]. Acta Metall. Sin., 2024, 60: 699
|
| [39] |
孟子凯, 孟智超, 高长源 等. 不同条件下纳米晶α-Zr蠕变行为的分子动力学模拟 [J]. 金属学报, 2024, 60: 699
doi: 10.11900/0412.1961.2022.00444
|
| [40] |
Yi X N, Ma A L, Zhang L M, et al. Crystallographic anisotropy of corrosion rate and surface faceting of polycrystalline 90Cu-10Ni in acidic NaCl solution [J]. Mater. Des., 2022, 215: 110429
doi: 10.1016/j.matdes.2022.110429
|
| [41] |
Yi X N, Zhang L J, Ma A L, et al. Study on anisotropic oxide formation rate in the initial corrosion stage of 90Cu-10Ni alloy in alkaline NaCl solution by experiments and first-principles calculation [J]. Corros. Sci., 2022, 209: 110768
doi: 10.1016/j.corsci.2022.110768
|
| [42] |
Kong M, Wu J J, Han T R, et al. Corrosion mechanism of T1 phase in Al-Cu-Li alloy: First-principles calculations [J]. Acta Phys. Sin., 2020, 69: 027101
|
| [42] |
孔 敏, 吴静静, 韩天茹 等. 第一性原理研究Al-Cu-Li合金中T1相的腐蚀机理 [J]. 物理学报, 2020, 69: 027101
|
| [43] |
Shin D Y, Lim D H. DFT approach for predicting the pH-potential-dependent durabilities of Pt-skinned Pt-M (M = Ni, Co, and Ir) alloys for fuel cell cathodes [J]. Appl. Surf. Sci., 2023, 616: 156449
doi: 10.1016/j.apsusc.2023.156449
|
| [44] |
Hu S B, Liu L, Cui Y, et al. Influence of hydrostatic pressure on the corrosion behavior of 90/10 copper-nickel alloy tube under alternating dry and wet condition [J]. Corros. Sci., 2019, 146: 202
doi: 10.1016/j.corsci.2018.10.036
|
| [45] |
Oktavian R, Taha M, Lee M J. Experimental and computational study of CO2 storage and sequestration with aqueous 2-amino-2-hydroxymethyl-1,3-propanediol (TRIS) solutions [J]. J. Phys. Chem., 2014, 118A: 11572
|
| [46] |
Liu B Y, Xi H X, Li Z, et al. Adsorption and corrosion-inhibiting effect of 2-(2-{[2-(4-Pyridylcarbonyl)hydrazono]methyl}phenoxy)acetic acid on mild steel surface in seawater [J]. Appl. Surf. Sci., 2012, 258: 6679
doi: 10.1016/j.apsusc.2012.03.115
|
| [47] |
Liu R, Cui Y, Liu L, et al. Study on the mechanism of hydrostatic pressure promoting electrochemical corrosion of pure iron in 3.5% NaCl solution [J]. Acta Mater., 2021, 203: 116467
doi: 10.1016/j.actamat.2020.11.009
|
| [48] |
Du J. Erosion-corrosion behavior of copper and 90/10 Cu-Ni alloy in flowing seawater [D]. Qingdao: Ocean University of China, 2007
|
| [48] |
杜 娟. TUP紫铜及B10铜镍合金流动海水冲刷腐蚀行为研究 [D]. 青岛: 中国海洋大学, 2007
|
| [49] |
Yi X N, Ma A L, Zheng Y G, et al. Elucidating different selective corrosion behavior of two typical marine aluminum bronze alloys from the perspective of constituent phases [J]. Corros. Sci., 2024, 235: 112167
doi: 10.1016/j.corsci.2024.112167
|
| [50] |
Tan Z W, Yang L Y, Zhang D L, et al. Development mechanism of internal local corrosion of X80 pipeline steel [J]. J. Mater. Sci. Technol., 2020, 49: 186
doi: 10.1016/j.jmst.2019.10.023
|
| [51] |
Yang L Y, Zhang D L, Fan H M, et al. In-situ electrochemical testing and fluid dynamics simulation of pipeline defects under flow accelerated corrosion [J]. Exp. Therm. Fluid Sci., 2024, 150: 111048
doi: 10.1016/j.expthermflusci.2023.111048
|
| [52] |
Liu Q, Zhao W N, Ao Z M, et al. Photo-piezoelectric synergistic degradation of typical volatile organic compounds on BaTiO3 [J]. Chin. Chem. Lett., 2022, 33: 410
doi: 10.1016/j.cclet.2021.06.059
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
| |
Shared |
|
|
|
|
| |
Discussed |
|
|
|
|