热成形汽车钢的弯曲韧性与氢脆行为研究进展
杜德灏1,2,3, 管明1,2, 曹祚恒1,2, 王铭1,2(), 何斌斌3, 黄明欣1,2()
1 香港大学 机械工程系 香港 999077
2 香港大学 深圳研究院 深圳 518057
3 南方科技大学 机械与能源工程系 深圳 518055
A Review of Current State and Prospects of the Bendability and Hydrogen Embrittlement Behavior of Press- Hardening Automobile Steels
DU Dehao1,2,3, GUAN Ming1,2, CAO Zuoheng1,2, WANG Ming1,2(), HE Binbin3, HUANG Mingxin1,2()
1 Department of Mechanical Engineering, University of Hong Kong, Hong Kong 999077, China
2 Shenzhen Institute of Research and Innovation, University of Hong Kong, Shenzhen 518057, China
3 Department of Mechanical and Energy Engineering, Southern University of Science and Technology, Shenzhen 518055, China
引用本文:

杜德灏, 管明, 曹祚恒, 王铭, 何斌斌, 黄明欣. 热成形汽车钢的弯曲韧性与氢脆行为研究进展[J]. 金属学报, 2026, 62(5): 959-974.
Dehao DU, Ming GUAN, Zuoheng CAO, Ming WANG, Binbin HE, Mingxin HUANG. A Review of Current State and Prospects of the Bendability and Hydrogen Embrittlement Behavior of Press- Hardening Automobile Steels[J]. Acta Metall Sin, 2026, 62(5): 959-974.

全文: PDF(3765 KB)   HTML
摘要: 

热成形钢以其高强度、优良的成形性能和能够制造出复杂几何形状零部件等优点,成为实现新能源汽车高安全性和轻量化的关键结构材料之一,广泛应用于汽车安全部件的制造。随着汽车工业对轻量化需求的不断增加,热成形钢正朝着更高强度、塑性和断裂韧性的方向发展。然而,在技术进步的同时,热成形钢在低弯曲韧性和氢脆方面面临的挑战也日益严峻。本文从三个方面总结了热成形钢断裂韧性和氢脆行为的最新研究进展:首先,介绍了热冲压工艺及具有高强韧性的最新热成形材料;其次,总结了当前商用热成形钢关于弯曲韧性的研究,结合材料表面镀层结构和弯曲角评价标准,探讨了镀层钢的结构局限性,并展望了提升镀层热成形钢弯曲性能的未来发展方向;最后,总结了热成形钢氢脆行为的研究进展。从氢脆的产生机理出发,分析并总结了材料内部微观结构和表面镀层等因素对热成形钢抗氢脆性能的影响,并对未来高强度热成形钢抗氢脆设计的研究方向进行展望。

关键词 : 热成形钢,  镀层,  弯曲韧性,  氢脆    
Abstract:

Press-hardening steel offers numerous advantages, such as exceptional strength, excellent formability, and the ability to produce complex geometries, making it an essential material for lightweight, high-performance structures in new-energy vehicles. Press-hardening steel is widely used in manufacturing safety components for vehicles. With the escalating demand for lightweight components in the automotive industry, press-hardening steel is evolving toward enhanced strength, ductility, and fracture toughness. However, alongside technological advancements, the challenges faced by press-hardening steel in terms of low bending toughness and hydrogen embrittlement are becoming increasingly severe. This review summarizes the current state and future prospects of press-hardening steel from three key perspectives. Firstly, it describes the press-hardening process and the development of advanced materials with enhanced strength and toughness. Secondly, it reviews recent research on toughening commercial press-hardening steels, examining the interplay between surficial steel coatings and cold-bending-angle standards, addressing the structural limitations of current products, and highlighting future advancements in coatings. Lastly, the paper summarizes the latest research on hydrogen embrittlement in press-hardening steel, starting with the underlying mechanisms of hydrogen-induced damage, while considering factors such as the internal microstructure and surface coating conditions of the steel. The paper concludes by outlining research directions for developing higher-strength press-hardening steels with improved resistance to hydrogen embrittlement.

Key words: press-hardening steel    coating    bendability    hydrogen embrittlement
收稿日期: 2025-09-14     
ZTFLH:  TG142  
基金资助:国家自然科学基金项目(52130102);国家自然科学基金项目(52425105);国家重点研发计划项目(2019YFA0209900);香港研究资助局项目(C7045-19E);香港研究资助局项目(R7066-18);创新及科技计划项目(MHP/064/20);新基石科学基金会设立的科学探索奖
通讯作者: 黄明欣,mxhuang@hku.hk,主要从事汽车用先进钢铁材料的设计与开发; 王 铭,mingwang@hku.hk,主要从事汽车用先进钢铁材料的设计与开发
Corresponding author: HUANG Mingxin, professor, Tel: (00852)39177906, E-mail: mxhuang@hku.hk; WANG Ming, research assistant professor, Tel: (00852)69931959, E-mail: mingwang@hku.hk
作者简介: 杜德灏,男,1995年生,博士生
图1  热冲压前后Al-Si镀层硼钢横截面分层结构的SEM像[5]
SteelChemical composition (mass fraction / %)Tensile strength MPa
CMnBSiCrTiNbVMo
22MnB5[11]0.231.180.0020.220.160.040---1478
25MnB5[11]0.251.240.0020.210.340.042---1611
28MnB5[11]0.281.300.0050.40-----1740
30MnB5[14]0.301.580.0050.330.360.055-0.04-1880
32MnB5[12]0.321.200.0030.250.120.0300.05--1904
34MnB5[11]0.341.300.0050.40-----1919
35MnB5[13]0.361.400.0030.20-----2000
37MnB4[11]0.370.810.0010.310.190.046---2040
38MnB5[11]0.381.200.0030.190.280.024--0.0052181
表1  典型热成形钢的化学成分和抗拉强度[11~14]
图2  不同两步奥氏体化工艺下的镀层结构和弯曲断裂韧性[25]
图3  热冲压前后的热浸镀纯Zn (GI)镀层示意图及液态金属脆化(LME)过程[29]
图4  H在22MnB5钢中不同晶界上的分布规律[44]
图5  拉伸强度为1500和2000 MPa的热成形钢的断裂韧性和裂纹扩展行为[47]
图6  组织细化对1800 MPa热成形钢微观组织和抗氢脆性能的影响[61]
图7  NbC对高强度马氏体钢抗氢脆性能的影响[63]
图8  夹杂物对氢脆的影响[71,74]
图9  锌镀层对热成形钢氢脆风险的影响[8,85]
[1] Li J, Lu H Z, Yi H L, et al. Lightweight of Passenger Car and Niobium-Microalloying Steel [M]. Beijing: Beijing Institute of Technology Press, 2015: 3
[1] 李 军, 路洪洲, 易红亮 等. 乘用车轻量化及微合金化钢板的应用 [M]. 北京: 北京理工大学出版社, 2015: 3
[2] Taylor T, Clough A. Critical review of automotive hot-stamped sheet steel from an industrial perspective [J]. Mater. Sci. Technol., 2018, 34: 809
doi: 10.1080/02670836.2018.1425239
[3] Wang Z, Xu N A, Huang M X. Phase transformation and carbon profile at the interface between Al-Si coating and steel substrate in a press-hardened steel [J]. Materialia, 2021, 20: 101268
doi: 10.1016/j.mtla.2021.101268
[4] Zhang Y Q, Zhang X, Sheng G, et al. Effect of ultra-fine martensite and retained austenite induced by slow quenching on the mechanical properties of 9Cr1.5Mo1Co(FB2) steel [J]. Mater. Charact., 2021, 181: 111452
doi: 10.1016/j.matchar.2021.111452
[5] Gui Z X, Wang K, Zhang Y S, et al. Cracking and interfacial debonding of the Al-Si coating in hot stamping of pre-coated boron steel [J]. Appl. Surf. Sci., 2014, 316: 595
doi: 10.1016/j.apsusc.2014.08.043
[6] Zhang J, Jiang S M, Zhang Q F, et al. Effect of temperature on microstructure and formability of Al-10 mass% Si coatings [J]. J. Iron Steel Res. Int., 2016, 23: 270
[7] Yuan X H, Zhang Q F. Microstructure evolution of hot-dip Al-10%Si coating during the austenitization of 22MnB5 hot stamping steel [J]. Acta Metall. Sin., 2017, 53: 1495
doi: 10.11900/0412.1961.2017.00077
[7] 袁训华, 张启富. 22MnB5热成形钢奥氏体化时热镀Al-10%Si镀层组织的演化 [J]. 金属学报, 2017, 53: 1495
doi: 10.11900/0412.1961.2017.00077
[8] Jo K R, Cho L, Sulistiyo D H, et al. Effects of Al-Si coating and Zn coating on the hydrogen uptake and embrittlement of ultra-high strength press-hardened steel [J]. Surf. Coat. Technol., 2019, 374: 1108
doi: 10.1016/j.surfcoat.2019.06.047
[9] Lee C W, Fan D W, Sohn I R, et al. Liquid-metal-induced embrittlement of Zn-coated hot stamping steel [J]. Metall. Mater. Trans., 2012, 43A: 5122
[10] Maki T, Tsuzaki K, Tamura I. The morphology of microstructure composed of lath martensites in steels [J]. Trans. Iron Steel Inst. Jpn., 1980, 20: 207
doi: 10.2355/isijinternational1966.20.207
[11] Rana R, Singh S B. Automotive Steels: Design, Metallurgy, Processing and Applications [M]. Cambridge: Woodhead Publishing, 2016: 1
[12] Yoo J, Jo M C, Bian J, et al. Effects of Nb or (Nb + Mo) alloying on charpy impact, bending, and delayed fracture properties in 1.9-GPa-grade press hardening steels [J]. Mater. Charact., 2021, 176: 111133
doi: 10.1016/j.matchar.2021.111133
[13] Chang Z Y, Li Y J, Wu D. Enhanced ductility and toughness in 2000 MPa grade press hardening steels by auto-tempering [J]. Mater. Sci. Eng., 2020, A784: 139342
[14] Cheng Z, Wang S Z, Liu J Y, et al. Precipitation behaviour and strengthening mechanisms of V-bearing 1800 MPa grade hot-stamping steel [J]. Mater. Sci. Technol., 2023, 39: 1592
doi: 10.1080/02670836.2023.2176621
[15] Lin L, Li B S, Zhu G M, et al. Effect of niobium precipitation behavior on microstructure and hydrogen induced cracking of press hardening steel 22MnB5 [J]. Mater. Sci. Eng., 2018, A721: 38
[16] Yi H L, Chang Z Y, Cai H L, et al. Strength, ductility and fracture strain of press-hardening steels [J]. Acta Metall. Sin., 2020, 56: 429
[16] 易红亮, 常智渊, 才贺龙 等. 热冲压成形钢的强度与塑性及断裂应变 [J]. 金属学报, 2020, 56: 429
doi: 10.11900/0412.1961.2020.00003
[17] Wei X L, Chai Z S, Lu Q, et al. Cr-alloyed novel press-hardening steel with superior combination of strength and ductility [J]. Mater. Sci. Eng., 2021, A819: 141461
[18] Hou Z R, Min J Y, Wang J F, et al. Effect of rapid heating on microstructure and tensile properties of a novel coating-free oxidation-resistant press-hardening steel [J]. JOM, 2021, 73: 3195
doi: 10.1007/s11837-021-04877-7
[19] Xie Z D, Ding C C, Wen P Y, et al. Effect of flash heating on microstructure and mechanical properties of 2000 MPa hot stamping steel [J]. Acta Metall. Sin., 2024, 60: 1667
doi: 10.11900/0412.1961.2023.00036
[19] 谢泽东, 丁灿灿, 温鹏宇 等. 闪速加热对2000 MPa级热成形钢显微组织和力学性能的影响 [J]. 金属学报, 2024, 60: 1667
doi: 10.11900/0412.1961.2023.00036
[20] Lu Q, Lai Q Q, Chai Z S, et al. Revolutionizing car body manufacturing using a unified steel metallurgy concept [J]. Sci. Adv., 2021, 7: eabk0176
doi: 10.1126/sciadv.abk0176
[21] Liu H P, Lu X W, Jin X J, et al. Enhanced mechanical properties of a hot stamped advanced high-strength steel treated by quenching and partitioning process [J]. Scr. Mater., 2011, 64: 749
doi: 10.1016/j.scriptamat.2010.12.037
[22] Cai H L, Chen P, Oh J K, et al. Quenching and flash-partitioning enables austenite stabilization during press-hardening processing [J]. Scr. Mater., 2020, 178: 77
doi: 10.1016/j.scriptamat.2019.10.047
[23] Ding C C, Hu K H, Chen H, et al. A dual-phase press-hardening steel with improved mechanical properties and superior oxidation resistance [J]. Metall. Mater. Trans., 2022, 53A: 1934
[24] Wang Z, Cao Z H, Wang J F, et al. Improving the bending toughness of Al-Si coated press-hardened steel by tailoring coating thickness [J]. Scr. Mater., 2021, 192: 19
doi: 10.1016/j.scriptamat.2020.10.008
[25] Guan M, Wang Y, Liu Y X, et al. Optimizing bendability of alsi-coated 2GPa-grade press-hardened steel by double austenitization [J]. Scr. Mater., 2023, 235: 115640
doi: 10.1016/j.scriptamat.2023.115640
[26] Yoo J, Kim S, Jo M C, et al. Effects of Al-Si coating structures on bendability and resistance to hydrogen embrittlement in 1.5-GPa-grade hot-press-forming steel [J]. Acta Mater., 2022, 225: 117561
doi: 10.1016/j.actamat.2021.117561
[27] Golem L, Cho L, Speer J G, et al. Influence of austenitizing parameters on microstructure and mechanical properties of Al-Si coated press hardened steel [J]. Mater. Des., 2019, 172: 107707
doi: 10.1016/j.matdes.2019.107707
[28] Bhattacharya D, Cho L, van der Aa E, et al. Transgranular cracking in a liquid Zn embrittled high strength steel [J]. Scr. Mater., 2020, 175: 49
doi: 10.1016/j.scriptamat.2019.09.006
[29] Billur E. Hot Stamping of Ultra High-Strength Steels: From A Technological and Business Perspective [M]. Cham: Springer, 2019: 1
[30] Bhattacharya D, Cho L, van der Aa E, et al. Influence of the starting microstructure of an advanced high strength steel on the characteristics of Zn-assisted liquid metal embrittlement [J]. Mater. Sci. Eng., 2021, A804: 140391
[31] Song M, Kim H, Lee S. Effect of a Zn interlayer on the adhesion strength and corrosion resistance of Zn-Mg coated TRIP steel [J]. ISIJ Int., 2019, 59: 1113
doi: 10.2355/isijinternational.ISIJINT-2018-476
[32] Cho L, Sulistiyo D H, Seo E J, et al. Hydrogen absorption and embrittlement of ultra-high strength aluminized press hardening steel [J]. Mater. Sci. Eng., 2018, A734: 416
[33] Shibata A, Yonemura T, Momotani Y, et al. Effects of local stress, strain, and hydrogen content on hydrogen-related fracture behavior in low-carbon martensitic steel [J]. Acta Mater., 2021, 210: 116828
doi: 10.1016/j.actamat.2021.116828
[34] Geng W T, Wang V, Li J X, et al. Hydrogen trapping in carbon supersaturated α iron and its decohesion effect in martensitic steel [J]. Scr. Mater., 2018, 149: 79
doi: 10.1016/j.scriptamat.2018.02.025
[35] Venezuela J, Zhou Q J, Liu Q L, et al. Influence of hydrogen on the mechanical and fracture properties of some martensitic advanced high strength steels in simulated service conditions [J]. Corros. Sci., 2016, 111: 602
doi: 10.1016/j.corsci.2016.05.040
[36] Depover T, Verbeken K. The effect of TiC on the hydrogen induced ductility loss and trapping behavior of Fe-C-Ti alloys [J]. Corros. Sci., 2016, 112: 308
doi: 10.1016/j.corsci.2016.07.013
[37] Chen Y S, Lu H Z, Liang J T, et al. Observation of hydrogen trapping at dislocations, grain boundaries, and precipitates [J]. Science, 2020, 367: 171
doi: 10.1126/science.aaz0122
[38] Takahashi J, Kawakami K, Kobayashi Y. Origin of hydrogen trapping site in vanadium carbide precipitation strengthening steel [J]. Acta Mater., 2018, 153: 193
doi: 10.1016/j.actamat.2018.05.003
[39] Zheng S Q, Qi Y M, Chen C F, et al. Effect of hydrogen and inclusions on the tensile properties and fracture behaviour of A350LF2 steels after exposure to wet H2S environments [J]. Corros. Sci., 2012, 60: 59
doi: 10.1016/j.corsci.2012.04.012
[40] Fujita S, Murakami Y. A new nonmetallic inclusion rating method by positive use of hydrogen embrittlement phenomenon [J]. Metall. Mater. Trans., 2013, 44A: 303
[41] Choi W S, De Cooman B C. Characterization of the bendability of press-hardened 22MnB5 steel [J]. Steel Res. Int., 2014, 85: 824
doi: 10.1002/srin.v85.5
[42] Li S S, Wen P Y, Li S L, et al. A novel medium-Mn steel with superior mechanical properties and marginal oxidization after press hardening [J]. Acta Mater., 2021, 205: 116567
doi: 10.1016/j.actamat.2020.116567
[43] Xu X X, Shen X Y, Wang J J, et al. YAP prevents premature senescence of astrocytes and cognitive decline of Alzheimer's disease through regulating CDK6 signaling [J]. Aging Cell, 2021, 20: e13465
doi: 10.1111/acel.v20.9
[44] Ngiam Y, Cao Z H, Huang M X. Understanding hydrogen embrittlement in press-hardened steel by coupling phase field and hydrogen diffusion modeling [J]. Mater. Sci. Eng., 2022, A834: 142523
[45] Cao Z H, Ngiam Y, Huang C P, et al. On the hydrogen embrittlement mechanism of 2 GPa-grade press-hardened steel at various strain rates: Experiments and modeling [J]. J. Mater. Sci. Technol., 2025, 224: 142
doi: 10.1016/j.jmst.2024.11.006
[46] Lin Y C, McCarroll I E, Lin Y T, et al. Hydrogen trapping and desorption of dual precipitates in tempered low-carbon martensitic steel [J]. Acta Mater., 2020, 196: 516
doi: 10.1016/j.actamat.2020.06.046
[47] Cao Z H, Zhang B N, Huang M X. Comparing hydrogen embrittlement behaviors of two press hardening steels: 2 GPa vs. 1.5 GPa grade [J]. J. Mater. Sci. Technol., 2022, 124: 109
doi: 10.1016/j.jmst.2022.02.020
[48] Zhu X, Li W, Hsu T Y, et al. Improved resistance to hydrogen embrittlement in a high-strength steel by quenching-partitioning-tempering treatment [J]. Scr. Mater., 2015, 97: 21
doi: 10.1016/j.scriptamat.2014.10.030
[49] Bhadeshia H K D H. Prevention of hydrogen embrittlement in steels [J]. ISIJ Int., 2016, 56: 24
doi: 10.2355/isijinternational.ISIJINT-2015-430
[50] Zhao W H, Liu J, Wang B Y, et al. A phase 1, open-label study of LCAR-B38M, a chimeric antigen receptor T cell therapy directed against B cell maturation antigen, in patients with relapsed or refractory multiple myeloma [J]. J. Hematol. Oncol., 2018, 11: 141
doi: 10.1186/s13045-018-0681-6
[51] Cho L, Bradley P E, Lauria D S, et al. Characteristics and mechanisms of hydrogen-induced quasi-cleavage fracture of lath martensitic steel [J]. Acta Mater., 2021, 206: 116635
doi: 10.1016/j.actamat.2021.116635
[52] Song Y S, Liao Y, Li C W, et al. Effects of reversed austenite on the cryogenic impact toughness of 0Cr16Ni5Mo1 super martensitic stainless steel [J]. Acta Metall. Sin., 2025, 61: 687
doi: 10.11900/0412.1961.2023.00100
[52] 宋逸思, 廖 瑜, 李传维 等. 逆转变奥氏体对0Cr16Ni5Mo1超级马氏体不锈钢低温冲击韧性的影响 [J]. 金属学报, 2025, 61: 687
doi: 10.11900/0412.1961.2023.00100
[53] Asari D, Mizokami S, Fukahori M, et al. Microscopic defects formed during crack incubation, initiation and propagation processes causing hydrogen-related fracture of dual-phase steels [J]. Mater. Sci. Eng., 2020, A780: 139209
[54] Wang Z, Huang M X. Optimising the strength-ductility-toughness combination in ultra-high strength quenching and partitioning steels by tailoring martensite matrix and retained austenite [J]. Int. J. Plast., 2020, 134: 102851
doi: 10.1016/j.ijplas.2020.102851
[55] Sun B H, Wang D, Lu X, et al. Current challenges and opportunities toward understanding hydrogen embrittlement mechanisms in advanced high-strength steels: A review [J]. Acta Metall. Sin. (Engl. Lett.), 2021, 34: 741
doi: 10.1007/s40195-021-01233-1
[56] Li Y J, Ponge D, Choi P, et al. Segregation of boron at prior austenite grain boundaries in a quenched martensitic steel studied by atom probe tomography [J]. Scr. Mater., 2015, 96: 13
doi: 10.1016/j.scriptamat.2014.09.031
[57] Miyamoto G, Goto A, Takayama N, et al. Three-dimensional atom probe analysis of boron segregation at austenite grain boundary in a low carbon steel—Effects of boundary misorientation and quen-ching temperature [J]. Scr. Mater., 2018, 154: 168
doi: 10.1016/j.scriptamat.2018.05.046
[58] Sun B H, Palanisamy D, Ponge D, et al. Revealing fracture mechanisms of medium manganese steels with and without delta-ferrite [J]. Acta Mater., 2019, 164: 683
doi: 10.1016/j.actamat.2018.11.029
[59] Shi H, Hachet G, Cheng H J, et al. Improving hydrogen embrittlement resistance of martensitic steel via interface B segregation [J]. Int. J. Hydrogen Energy, 2025, 164: 150954
doi: 10.1016/j.ijhydene.2025.150954
[60] Hachet G, Wei S L, Tehranchi A, et al. Protection of metal interfaces against hydrogen-assisted cracking [J]. Nat. Commun., 2025, 16: 11032
doi: 10.1038/s41467-025-67310-6
[61] Du D H, Zhang Y, Geng Z Y, et al. Improving the hydrogen embrittlement property of 1.8 GPa press-hardened steel by controlling the prior austenite grain size [J]. Metall. Mater. Trans., 2024, 55A: 2940
[62] Kirchheim R. Changing the interfacial composition of carbide precipitates in metals and its effect on hydrogen trapping [J]. Scr. Mater., 2019, 160: 62
doi: 10.1016/j.scriptamat.2018.09.043
[63] Shi R J, Ma Y, Wang Z D, et al. Atomic-scale investigation of deep hydrogen trapping in NbC/α-Fe semi-coherent interfaces [J]. Acta Mater., 2020, 200: 686
doi: 10.1016/j.actamat.2020.09.031
[64] Yoo J, Jo M C, Kim D W, et al. Effects of Cu addition on resistance to hydrogen embrittlement in 1 GPa-grade duplex lightweight steels [J]. Acta Mater., 2020, 196: 370
doi: 10.1016/j.actamat.2020.06.051
[65] Wei F G, Tsuzaki K. Hydrogen absorption of incoherent TiC particles in iron from environment at high temperatures [J]. Metall. Mater. Trans., 2004, 35A: 3155
[66] Hong S G, Kang K B, Park C G. Strain-induced precipitation of NbC in Nb and Nb-Ti microalloyed HSLA steels [J]. Scr. Mater., 2002, 46: 163
doi: 10.1016/S1359-6462(01)01214-3
[67] Nagao A, Martin M L, Dadfarnia M, et al. The effect of nanosized (Ti, Mo)C precipitates on hydrogen embrittlement of tempered lath martensitic steel [J]. Acta Mater., 2014, 74: 244
doi: 10.1016/j.actamat.2014.04.051
[68] Yoo J, Jo M C, Jo M C, et al. Effects of Ti alloying on resistance to hydrogen embrittlement in (Nb + Mo)-alloyed ultra-high-strength hot-stamping steels [J]. Mater. Sci. Eng., 2020, A791: 139763
[69] Zhang B N, Su J, Wang M Q, et al. Atomistic insight into hydrogen trapping at MC/BCC-Fe phase boundaries: The role of local atomic environment [J]. Acta Mater., 2021, 208: 116744
doi: 10.1016/j.actamat.2021.116744
[70] Jakob S, Sattari M, Sefer B, et al. Characterization of hydrogen traps in a co-precipitation steel investigated by atom probe experiments without cryogenic transfer [J]. Scr. Mater., 2024, 243: 115963
doi: 10.1016/j.scriptamat.2023.115963
[71] Wang Z, Lu Q, Cao Z H, et al. Review on hydrogen embrittlement of press-hardened steels for automotive applications [J]. Acta Metall. Sin. (Engl. Lett.), 2023, 36: 1123
doi: 10.1007/s40195-022-01408-4
[72] Depover T, Monbaliu O, Wallaert E, et al. Effect of Ti, Mo and Cr based precipitates on the hydrogen trapping and embrittlement of Fe-C-X Q&T alloys [J]. Int. J. Hydrogen Energy, 2015, 40: 16977
doi: 10.1016/j.ijhydene.2015.06.157
[73] Cho L, Bradley P E, Lauria D S, et al. Effects of hydrogen pressure and prior austenite grain size on the hydrogen embrittlement characteristics of a press-hardened martensitic steel [J]. Int. J. Hydrogen Energy, 2021, 46: 24425
doi: 10.1016/j.ijhydene.2021.05.005
[74] Garet M, Brass A M, Haut C, et al. Hydrogen trapping on non metallic inclusions in Cr-Mo low alloy steels [J]. Corros. Sci., 1998, 40: 1073
doi: 10.1016/S0010-938X(98)00008-0
[75] Laureys A, van den Eeckhout E, Petrov R, et al. Effect of deformation and charging conditions on crack and blister formation during electrochemical hydrogen charging [J]. Acta Mater., 2017, 127: 192
doi: 10.1016/j.actamat.2017.01.013
[76] Peng Z X, Liu J, Huang F, et al. Effect of submicron‐scale MnS inclusions on hydrogen trapping and hic susceptibility of X70 pipeline steels [J]. Steel Res. Int., 2018, 89: 1700566
doi: 10.1002/srin.v89.7
[77] Pallaspuro S, Fangnon E, Aravindh S A, et al. Mitigating hydrogen embrittlement via film-like retained austenite in 2 GPa direct-quenched and partitioned martensitic steels [J]. Mater. Sci. Eng., 2024, A908: 146872
[78] Turk A, Pu S D, Bombač D, et al. Quantification of hydrogen trapping in multiphase steels: Part II-effect of austenite morphology [J]. Acta Mater., 2020, 197: 253
doi: 10.1016/j.actamat.2020.07.039
[79] Du D H, Guan M, Cao Z H, et al. Alleviating strength-hydrogen embrittlement trade-off in TRIP1180 steel via vanadium carbide reinforced ferrite matrix [J]. Scr. Mater., 2026, 271: 117045
doi: 10.1016/j.scriptamat.2025.117045
[80] Wang L, Speer J G. Quenching and partitioning steel heat treatment [J]. Metallogr., Microstruct., Anal., 2013, 2: 268
[81] Sun B H, Lu W J, Gault B, et al. Chemical heterogeneity enhances hydrogen resistance in high-strength steels [J]. Nat. Mater., 2021, 20: 1629
doi: 10.1038/s41563-021-01050-y pmid: 34239084
[82] Xiong Z P, Jacques P J, Perlade A, et al. Ductile and intergranular brittle fracture in a two-step quenching and partitioning steel [J]. Scr. Mater., 2018, 157: 6
doi: 10.1016/j.scriptamat.2018.07.030
[83] Deng Y, Barnoush A. Hydrogen embrittlement revealed via novel in situ fracture experiments using notched micro-cantilever specimens [J]. Acta Mater., 2018, 142: 236
doi: 10.1016/j.actamat.2017.09.057
[84] Guan M, Zhang J Y, Wang Z, et al. Mitigating delayed fracture in AlSi-coated 2 GPa press-hardened steel via surface plasticity-induced hydrogen delocalization [J]. Acta Mater., 2025, 301: 121614
doi: 10.1016/j.actamat.2025.121614
[85] Reumont G, Vogt J B, Iost A, et al. The effects of an Fe-Zn intermetallic-containing coating on the stress corrosion cracking behavior of a hot-dip galvanized steel [J]. Surf. Coat. Technol., 2001, 139: 265
doi: 10.1016/S0257-8972(01)01017-9
[1] 宝尔根, 王建韬, 徐文静, 马会, 陈星秋. 合金元素对 α-Fe中H原子溶解及扩散影响的第一性原理研究[J]. 金属学报, 2026, 62(3): 489-496.
[2] 杨波, 陈小亮, 史晓斌, 任伟, 高恒, 宋广生. 稀土Y掺杂V-Cr合金增塑机理及透氢性能[J]. 金属学报, 2025, 61(6): 887-899.
[3] 顾天真, 刘雨薇, 彭灿, 张鹏, 王振尧, 汪川, 马成, 曹宏玮. Zn-2.0Al-1.5Mg镀层在模拟海洋大气中的腐蚀行为[J]. 金属学报, 2025, 61(2): 278-286.
[4] 谢泽东, 丁灿灿, 温鹏宇, 罗海文. 闪速加热对2000 MPa级热成形钢显微组织和力学性能的影响[J]. 金属学报, 2024, 60(12): 1667-1677.
[5] 肖娜, 惠卫军, 张永健, 赵晓丽. 真空渗碳处理齿轮钢的氢脆敏感性[J]. 金属学报, 2021, 57(8): 977-988.
[6] 兰亮云, 孔祥伟, 邱春林, 杜林秀. 基于多尺度力学实验的氢脆现象的最新研究进展[J]. 金属学报, 2021, 57(7): 845-859.
[7] 金学军,龚煜,韩先洪,杜浩,丁伟,朱彬,张宜生,冯毅,马鸣图,梁宾,赵岩,李勇,郑菁桦,石朱生. 先进热成形汽车钢制造与使用的研究现状与展望[J]. 金属学报, 2020, 56(4): 411-428.
[8] 易红亮,常智渊,才贺龙,杜鹏举,杨达朋. 热冲压成形钢的强度与塑性及断裂应变[J]. 金属学报, 2020, 56(4): 429-443.
[9] 李金许,王伟,周耀,刘神光,付豪,王正,阚博. 汽车用先进高强钢的氢脆研究进展[J]. 金属学报, 2020, 56(4): 444-458.
[10] 刘振宝,梁剑雄,苏杰,王晓辉,孙永庆,王长军,杨志勇. 高强度不锈钢的研究及发展现状[J]. 金属学报, 2020, 56(4): 549-557.
[11] 胡宽辉, 毛新平, 周桂峰, 刘静, 王志奋. Si和Mn含量对超高强度热成形钢组织和性能的影响[J]. 金属学报, 2018, 54(8): 1105-1112.
[12] 赵晓丽, 张永健, 邵成伟, 惠卫军, 董瀚. 两相区退火处理冷轧0.1C-5Mn中锰钢的氢脆敏感性[J]. 金属学报, 2018, 54(7): 1031-1041.
[13] 郭腾, 李洪涛, 蒋百灵, 邢益彬, 张新宇. 离子镀过程中基体“热影响区”的演变及其对镀层的影响[J]. 金属学报, 2018, 54(3): 463-469.
[14] 孙军, 李苏植, 丁向东, 李巨. 氢化空位的基本性质及其对金属力学行为的影响[J]. 金属学报, 2018, 54(11): 1683-1692.