| Orientation Selection Behavior During Secondary Recrystallization in Grain-Oriented Silicon Steel |
XU Zhanyi1, SHA Yuhui1( ), ZHANG Fang1, ZHANG Huabing2, LI Guobao2, CHU Shuangjie2, ZUO Liang1,3 |
1 Key Laboratory for Anisotropy and Texture of Materials, Ministry of Education, Northeastern University, Shenyang 110819, China 2 Baoshan Iron & Steel Cooperation Limited, Shanghai 201900, China 3 Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China |
|
Cite this article:
XU Zhanyi, SHA Yuhui, ZHANG Fang, ZHANG Huabing, LI Guobao, CHU Shuangjie, ZUO Liang. Orientation Selection Behavior During Secondary Recrystallization in Grain-Oriented Silicon Steel. Acta Metall Sin, 2020, 56(8): 1067-1074.
|
|
|
Abstract The key index of grain-oriented silicon steel is the sharpness of secondary recrystallization Goss ({110}<001>) texture, which is determined by the matrix grain size distribution, texture environment and inhibitor level. In the widely used low-temperature slab heating process in virtue of high efficiency and low-cost manufacturing, the instability of inhibitor and the enlarged matrix grain size distribution seriously restrict the occurrence of secondary recrystallization and the sharpness of Goss texture. The investigation on orientation selection behavior during abnormal grain growth can explore the potential routines to solve the problem. In this work, the evolution process of secondary recrystallization texture in grain-oriented silicon steel has been studied by both experiment and calculation. It is found that single Goss texture is finally obtained by means of continuous orientation selection during secondary recrystallization. The kinetic model for secondary recrystallization, introduced with orientation-dependent relative grain boundary energy coefficient, can describe quantitatively the difference in growth rate between Goss grains with various deviation angles and non-Goss grains. The combined effects of grain size distribution, grain boundary characteristic between Goss and matrix grains, together with inhibition force level on orientation selection behavior are analyzed. Accordingly, a multi-parameter matching method for promoting the advantage of Goss grains in orientation selection is proposed.
|
|
Received: 17 December 2019
|
|
|
| Fund: National Key Research and Development Program of China(2016YFB0300305);National Natural Science Foundation of China(51671049);National Natural Science Foundation of China(51931002) |
| [1] |
Hayakawa Y. Mechanism of secondary recrystallization of Goss grains in grain-oriented electrical steel [J]. Sci. Technol. Adv. Mater., 2017, 18: 480
doi: 10.1080/14686996.2017.1341277
pmid: 28804524
|
| [2] |
Xia Z S, Kang Y L, Wang Q L. Developments in the production of grain-oriented electrical steel [J]. J. Magn. Magn. Mater., 2008, 320: 3229
doi: 10.1016/j.jmmm.2008.07.003
|
| [3] |
Moses A J. Energy efficient electrical steels: Magnetic performance prediction and optimization [J]. Scr. Mater., 2012, 67: 560
doi: 10.1016/j.scriptamat.2012.02.027
|
| [4] |
He C X, Yang F Y, Yan G C, et al. Effect of normalizing on textures of thin-gauge grain-oriented silicon steel [J]. Acta Metall. Sin., 2016, 52: 1063
doi: 10.11900/0412.1961.2015.00554
|
|
(何承绪, 杨富尧, 严国春等. 常化处理对薄规格取向硅钢织构的影响 [J]. 金属学报, 2016, 52: 1063)
doi: 10.11900/0412.1961.2015.00554
|
| [5] |
Chu S J, Yang Y J, He Z H, et al. Calculation of magnetostriction coefficient for laser-scribed grain-oriented silicon steel based on magnetic domain interaction [J]. Acta Metall. Sin., 2019, 55: 362
doi: 10.11900/0412.1961.2018.00242
|
|
(储双杰, 杨勇杰, 和正华等. 基于磁畴结构交互作用的激光刻痕取向硅钢磁致伸缩系数计算 [J]. 金属学报, 2019, 55: 362)
doi: 10.11900/0412.1961.2018.00242
|
| [6] |
Ushigami Y, Mizokami M, Fujikura M, et al. Recent development of low-loss grain-oriented silicon steel [J]. J. Magn. Magn. Mater., 2003, 254-255: 307
doi: 10.1016/S0304-8853(02)00933-2
|
| [7] |
Harase J, Shimizu R. Distribution of {110}<001> oriented grains in the primary recrystallized 3% Si-Fe alloy [J]. Trans. Jpn. Inst. Met., 1988, 29(5): 388
doi: 10.2320/matertrans1960.29.388
|
| [8] |
Hayakawa Y, Szpunar J A, Palumbo G, et al. The role of grain boundary character distribution in Goss texture development in electrical steels [J]. J. Magn. Magn. Mater., 1996, 160: 143
doi: 10.1016/0304-8853(96)00141-2
|
| [9] |
Rouag N, Vigna G, Penelle R. Evolution of local texture and grain boundary characteristics during secondary recrystallisation of Fe-3%Si sheets [J]. Acta Metall. Mater., 1990, 38: 1101
doi: 10.1016/0956-7151(90)90182-G
|
| [10] |
Shimizu R, Harase J. Coincidence grain boundary and texture evolution in Fe-3%Si [J]. Acta Mater., 1989, 37: 1241
doi: 10.1016/0001-6160(89)90118-1
|
| [11] |
Lin P, Palumbo G, Harase J, et al. Coincidence site lattice (CSL) grain boundaries and Goss texture development in Fe-3%Si alloy [J]. Acta Mater., 1996, 44: 4677
doi: 10.1016/S1359-6454(96)00140-1
|
| [12] |
Kumano T, Ushigami Y. Grain boundary characteristics of isolated grains in conventional grain oriented silicon steel [J]. ISIJ Int., 2007, 47: 890
doi: 10.2355/isijinternational.47.890
|
| [13] |
Hayakawa Y, Szpunar J A. The role of grain boundary character distribution in secondary recrystallization of electrical steels [J]. Acta Mater., 1997, 45: 1285
doi: 10.1016/S1359-6454(96)00251-0
|
| [14] |
Hayakawa Y, Szpunar J A. A new model of Goss texture development during secondary recrystallization of electrical steel [J]. Acta Mater., 1997, 45: 4713
doi: 10.1016/S1359-6454(97)00111-0
|
| [15] |
Rajmohan N, Szpunar J A, Hayakawa Y. A role of fractions of mobile grain boundaries in secondary recrystallization of Fe-Si steels [J]. Acta Mater., 1999, 47: 2999
doi: 10.1016/S1359-6454(99)00162-7
|
| [16] |
Rajmohan N, Szpunar J A, Hayakawa Y. Importance of fractions of highly mobile boundaries in abnormal growth of Goss grains [J]. Mater. Sci. Eng., 1999, A259: 8
|
| [17] |
Rajmohan N, Szpunar J A. An analytical method for characterizing grain boundaries around growing Goss grains during secondary recrystallization [J]. Scr. Mater., 2001, 44: 2387
doi: 10.1016/S1359-6462(01)00941-1
|
| [18] |
Morawiec A. Grain misorientations in theories of abnormal grain growth in silicon steel [J]. Scr. Mater., 2000, 43: 275
doi: 10.1016/S1359-6462(00)00403-6
|
| [19] |
Morawiec A. On abnormal growth of Goss grains in grain-oriented silicon steel [J]. Scr. Mater., 2011, 64: 466
doi: 10.1016/j.scriptamat.2010.11.013
|
| [20] |
Nakayama T, Ushigami Y. Modeling of secondary recrystallization in 3% silicon steels [J]. Mater. Sci. Forum, 1992, 94-96: 413
doi: 10.4028/www.scientific.net/MSF.94-96
|
| [21] |
Ushigami Y, Kawasaki K, Nakayama T, et al. Dynamic observation of the growth of secondary recrystallized grains of Fe-3%Si alloy utilizing synchrotron X-ray topography [J]. Mater. Sci. Forum, 1994, 157-162: 1081
doi: 10.4028/www.scientific.net/MSF.157-162
|
| [22] |
Ushigami Y. Theoretical analysis and computer simulation of secondary recrystallization in grain-oriented silicon steel [R]. Nippon Steel Technical Report No.102, 2013: 25
|
| [23] |
Hillert M. On the theory of normal and abnormal grain growth [J]. Acta Metall., 1965, 13: 227
doi: 10.1016/0001-6160(65)90200-2
|
| [24] |
Furtkamp M, Gottstein G, Molodov D A, et al. Grain boundary migration in Fe-3.5%Si bicrystals with [001] tilt boundaries [J]. Acta Mater., 1998, 46: 4103
doi: 10.1016/S1359-6454(98)00105-0
|
| [25] |
Humphreys F J, Hatherly M. Recrystallization and Related Annealing Phenomena [M]. 2nd Ed., Amsterdam: Elsevier, 2004: 102
|
| [26] |
Liu G T, Liu Z Q, Yang P, et al. Correlation between primary and secondary recrystallization texture components in low-temperature reheated grain-oriented silicon steel [J]. J. Iron Steel Res. Int., 2016, 23: 1234
doi: 10.1016/S1006-706X(16)30181-9
|
| [27] |
Yoshitomi Y, Ushigami Y, Harase J, et al. Coincidence grain boundary and role of primary recrystallized grain growth on secondary recrystallization texture evolution in Fe-3%Si alloy [J]. Acta Metall. Mater., 1994, 42: 2593
doi: 10.1016/0956-7151(94)90200-3
|
| [28] |
Ko K J, Rollett A D, Hwang N M. Abnormal grain growth of Goss grains in Fe-3%Si steel driven by sub-boundary-enhanced solid-state wetting: Analysis by Monte Carlo simulation [J]. Acta Mater., 2010, 58: 4414
doi: 10.1016/j.actamat.2010.04.038
|
| [29] |
Mao W M, Zhang M H, Yang P. Behaviors of normal grain growth in polycrystalline Fe-3%Si alloys [J]. Steel Res. Int., 2014, 85: 1215
doi: 10.1002/srinv85.7
|
| No Suggested Reading articles found! |
|
|