固溶处理对Cr-Ni-Co-Mo马氏体时效不锈钢显微组织及耐腐蚀性能的影响
杨佳伟1, 周德凯1, 赵利媛1, 王天宇1, 李小琳1(), 杨洪波2, 王海丰1()
1 西北工业大学 材料学院 凝固技术全国重点实验室 西安 710072
2 西安建筑科技大学 冶金工程学院 西安 710055
Effect of Solution Treatment on Microstructure and Corrosion Resistance of Cr-Ni-Co-Mo Maraging Stainless Steel
YANG Jiawei1, ZHOU Dekai1, ZHAO Liyuan1, WANG Tianyu1, LI Xiaolin1(), YANG Hongbo2, WANG Haifeng1()
1 State Key Laboratory of Solidification Processing, School of Materials Science and Engineering, Northwestern Polytechnical University, Xi'an 710072, China
2 School of Metallurgical Engineering, Xi'an University of Architecture and Technology, Xi'an 710055, China
引用本文:

杨佳伟, 周德凯, 赵利媛, 王天宇, 李小琳, 杨洪波, 王海丰. 固溶处理对Cr-Ni-Co-Mo马氏体时效不锈钢显微组织及耐腐蚀性能的影响[J]. 金属学报, 2025, 61(11): 1715-1726.
Jiawei YANG, Dekai ZHOU, Liyuan ZHAO, Tianyu WANG, Xiaolin LI, Hongbo YANG, Haifeng WANG. Effect of Solution Treatment on Microstructure and Corrosion Resistance of Cr-Ni-Co-Mo Maraging Stainless Steel[J]. Acta Metall Sin, 2025, 61(11): 1715-1726.

全文: PDF(4859 KB)   HTML
摘要: 

为了提高Cr-Ni-Co-Mo马氏体时效不锈钢的耐腐蚀性能,本工作设计了高温固溶+时效(HS)、低温固溶+时效(LS)和循环固溶+时效(CLS) 3种热处理工艺,研究了固溶处理方式对马氏体时效不锈钢晶粒尺寸、逆转变奥氏体体积分数的影响,并探究特征组织对马氏体时效不锈钢在3.5%NaCl (质量分数)溶液中的耐腐蚀性能的影响。结果表明,相比于高温固溶处理,低温固溶处理显著细化了马氏体板条块的尺寸(2.1 μm→943 nm),逆转变奥氏体体积分数增加至7.8%。循环固溶处理通过引入高密度位错和残余奥氏体,为时效过程中逆转变奥氏体的形成提供了形核位点和元素扩散通道,逆转变奥氏体体积分数提高至33%。周期浸润腐蚀实验表明,晶粒细化和逆转变奥氏体体积分数的增加显著提高了材料的耐腐蚀性能。晶粒细化通过增加晶界密度,促进表面钝化膜的形成,降低材料的晶间腐蚀敏感度。逆转变奥氏体通过增加钝化膜的稳定性和厚度,提高点蚀区的电荷转移电阻,显著增强了材料在含Cl⁻环境中的抗点蚀能力。

关键词 : 马氏体时效不锈钢,  晶粒细化,  逆转变奥氏体,  耐腐蚀机理    
Abstract:

Maraging stainless steel has extensive applications in aerospace, marine, and other demanding fields because of its high strength. However, its susceptibility to pitting corrosion in Cl--containing environments considerably limits its practical applications under corrosive conditions. This study investigates the effects of three solution treatments—high temperature solution (HS), low temperature solution (LS), and cyclic low temperature solution (CLS)—on grain size and reversed austenite formation in Cr-Ni-Co-Mo maraging stainless steel. Furthermore, it explores the relationship between its microstructure and corrosion resistance in a 3.5%NaCl (mass fraction) solution. The results revealed that the LS treatment refines the martensite block size from 2.1 μm to 943 nm and increases the reversed austenite content from 1.9% to 7.8% compared with the HS treatment. The CLS treatment introduces a high density of dislocations and retained austenite, which provide favorable nucleation sites and diffusion pathways for elemental redistribution during aging, thereby leading to a substantial increase in reversed austenite content to 33%. Cyclic infiltration corrosion tests and electrochemical measurements confirm that grain refinement and the enhanced reversed austenite content considerably improve the corrosion resistance. Grain refinement increases the density of grain boundaries, facilitates the formation of a passivation film on the surface and reduces susceptibility to intergranular corrosion. Compared with LS-treated steel, CLS-treated steel exhibits a 109 mVSCE increase in corrosion potential, an 86.25 μA/cm2 decrease in corrosion current density, and a 26.82 mVSCE increase in pitting potential. As the reversed austenite content increases, the total resistance of solution and the passivation film thickness increase, thereby improving the stability and protective performance of the passivation film. Concurrently, pitting charge transfer resistance increases, which improves resistance to pitting corrosion.

Key words: maraging stainless steel    grain refinement    reversed austenite    corrosion resistance mechanism
收稿日期: 2025-03-04     
ZTFLH:  TG142.24  
基金资助:国家重点研发计划项目(2022YFB3705300);国家自然科学基金项目(52374403);国家自然科学基金项目(U23A20613);国家自然科学基金项目(52004224);凝固技术全国重点实验室项目(2021-TS-10);西北工业大学研究生创新能力培育基金项目(PF2025040);分析测试中心研究基金项目(2023-T-009)
通讯作者: 李小琳,xiaolinli@nwpu.edu.cn,主要从事极端服役环境材料成分设计、组织调控及强韧化和腐蚀机理研究;
王海丰,haifengw81@nwpu.edu.cn,主要从事亚稳金属材料相变理论及金属材料开发应用研究
作者简介: 杨佳伟,男,2001年生,硕士生
图1  马氏体时效不锈钢的平衡相图、热膨胀曲线及热处理工艺流程示意图
图2  高温固溶+时效(HS)和低温固溶+时效(LS)试样的SEM像和XRD谱
图3  HS、LS试样及Cr-Ni-Co-Mo马氏体不锈钢[25]的TEM分析
图4  LS和循环固溶+时效(CLS)试样的EBSD分析
图5  低温固溶处理(LST)和循环固溶处理(CLST)试样的局部取向差(KAM)及其分布
图6  LST和CLST试样的XRD谱和相分布图
图7  各试样在3.5%NaCl (质量分数)溶液中的腐蚀速率
图8  HS和LS试样在3.5%NaCl溶液中循环284 cyc后的SEM像和EDS元素面扫描图
图9  CLS试样在3.5%NaCl溶液中循环284 cyc后的SEM像和EDS元素面扫描图
图10  LS和CLS样品在3.5%NaCl溶液中的腐蚀电化学性能
SampleEcorr / mVSCEicorr / (μA·cm-2)Epit / mVSCE
LS-253141.20-23.70
CLS-14454.953.12
表1  LS和CLS样品在3.5%NaCl溶液中的极化曲线特征参数
图11  马氏体时效不锈钢的等效电路图

Sample

Rpass

Ω·cm2

Rel

Ω·cm2

Rpit

Ω·cm2

CPEpassCPEpit

Y0-pass

μF·cm-2

bp

Y0-pass

μF·cm-2

bp
LS6.710.0112650029.30.9117.10.655
CLS15.603.3448540015.80.9092.90.571
表2  由等效电路拟合出的交流阻抗特征参数
图12  LS和CLS试样的总电阻和钝化膜厚度
[1] Guo L L, Zhang L N, Andersson J, et al. Additive manufacturing of 18% nickel maraging steels: Defect, structure and mechanical properties: A review [J]. J. Mater. Sci. Technol., 2022, 120: 227
[2] Tian Y, Palad R, Aranas Jr C. Microstructural evolution and mechanical properties of a newly designed steel fabricated by laser powder bed fusion [J]. Addit. Manuf., 2020, 36: 101495
[3] Man C, Dong C F, Kong D C, et al. Beneficial effect of reversed austenite on the intergranular corrosion resistance of martensitic stainless steel [J]. Corros. Sci., 2019, 151: 108
[4] Dos Santos Jr A G, Biehl L V, Antonini L M. Effect of chemical passivation treatment on pitting corrosion resistance of AISI 410 and 17-4 PH stainless steels [J]. Mater. Corros., 2017, 68: 824
[5] Tian J L, Li Y C, Wang W, et al. Alloying element segregation effect in a multi-phase strengthened maraging stainless steel [J]. Acta Metall. Sin., 2016, 52: 1517
[5] 田家龙, 李永灿, 王 威 等. 多相强化型马氏体时效不锈钢中的合金元素偏聚效应 [J]. 金属学报, 2016, 52: 1517
[6] Li Y T, Li X L, He Y, et al. Multiple oxidation mechanism of Al and Ti doping Haynes244 alloy under elevated temperature [J]. Surf. Coat. Technol., 2025, 498: 131826
[7] Si Y L, Xue J T, Wang X F, et al. Effect of Cr addition on the corrosion behavior of twinning-induced plasticity steel [J]. Acta Metall. Sin., 2023, 59: 905
[7] 司永礼, 薛金涛, 王幸福 等. Cr添加对孪生诱发塑性钢腐蚀行为的影响 [J]. 金属学报, 2023, 59: 905
[8] Chen Y, Gong C B, Wang S G, et al. Microstructure, microhardness, and corrosion properties of nanocrystalline 304 stainless steel plates [J]. Acta Metall. Sin., 10.11900/0412.1961.2024.00253
[8] 陈 园, 宫春波, 王胜刚 等. 纳米晶304不锈钢板材微观组织、显微硬度与腐蚀性能 [J]. 金属学报, 10.11900/0412.1961.2024.00253
[9] Wang X Y, Li D Y. Mechanical and electrochemical behavior of nanocrystalline surface of 304 stainless steel [J]. Electrochim. Acta, 2002, 47: 3939
[10] Meng G Z, Li Y, Wang F H. The corrosion behavior of Fe-10Cr nanocrystalline coating [J]. Electrochim. Acta, 2006, 51: 4277
[11] He L, Wu X Y, Zhang Z Y, et al. Microstructure evolution and corrosion behavior of duplex stainless steel during isothermal aged at 650 oC [J]. Int. J. Electrochem. Sci., 2016, 11: 8046
[12] Zhang W, Zhang X, Qiao G J, et al. Effect of cobalt on the microstructure and corrosion behavior of martensitic age-hardened stainless steel [J]. J. Mater. Eng. Perform., 2019, 28: 4197
[13] Wang P, Zheng W W, Dai X, et al. Prominent role of reversed austenite on corrosion property of super 13Cr martensitic stainless steel [J]. J. Mater. Res. Technol., 2023, 22: 1753
[14] Vishwakarma J, Chattopadhyay K, Santhi Srinivas N C. Influence of build orientation and aging on corrosion behaviour of 18Ni300 maraging steel produced via powder bed fusion using Laser beam (PBF-LB) [J]. Mater. Today Commun., 2023, 35: 105825
[15] Song X, Hu Y, Yan Z J, et al. Corrosion resistance improvement in 6Cr13 martensitic stainless steel via quenching-tempering and partitioning [J]. Mater. Corros., 2023, 74: 544
[16] Zhang H L, Sun M Y, Ma D P, et al. Effect of aging temperature on the heterogeneous microstructure and mechanical properties of a 12Cr-10Ni-Mo-Ti maraging steel for cryogenic applications [J]. J. Mater. Sci., 2021, 56: 11469
[17] Qiu X Y F, Yang Z Y, Ding Y L. Solid solution treatment for improving cryogenic temperature toughness of Cr-Ni-Mo-Ti maraging stainless steel [J]. Heat Treat. Met., 2022, 47: 44
[17] 邱旭扬帆, 杨卓越, 丁雅莉. 提高Cr-Ni-Mo-Ti马氏体时效不锈钢超低温韧性的固溶处理工艺 [J]. 金属热处理, 2022, 47: 44
[18] Zhang H L, Sun M Y, Liu Y X, et al. Ultrafine-grained dual-phase maraging steel with high strength and excellent cryogenic toughness [J]. Acta Mater., 2021, 211: 116878.
[19] Leem D S, Lee Y D, Jun J H, et al. Amount of retained austenite at room temperature after reverse transformation of martensite to austenite in an Fe-13%Cr-7%Ni-3%Si martensitic stainless steel [J]. Scr. Mater., 2001, 45: 767
[20] Jiang S H, Wang H, Wu Y, et al. Ultrastrong steel via minimal lattice misfit and high-density nanoprecipitation [J]. Nature, 2017, 544: 460
[21] Pereloma E V, Shekhter A, Miller M K, et al. Ageing behaviour of an Fe-20Ni-1.8Mn-1.6Ti-0.59Al (wt%) maraging alloy: Clustering, precipitation and hardening [J]. Acta Mater., 2004, 52: 5589
[22] Ding Y L, Gao Q, Wang A. Inheritance and refinement of coarse grains in hot forging rings of a Cr-Ni-Mo-Ti maraging stainless steel [J]. Heat Treat. Met., 2025, 50: 169
[22] 丁雅莉, 高 齐, 王 敖. Cr-Ni-Mo-Ti马氏体时效不锈钢热锻环粗晶粒的遗传及细化 [J]. 金属热处理, 2025, 50: 169
[23] Zhou X L, Jia C N, Mi P, et al. Cyclic quenching treatment doubles the Charpy V-notch impact energy of a 2.3 GPa maraging steel [J]. J. Mater. Sci. Technol., 2025, 209: 311
[24] Zhao L Y, Yang J W, Tian L, et al. The influence of tempering parameters on the microstructure, mechanical property, and the corresponding strengthening mechanism of metastable 301 austenitic stainless steel [J]. Steel Res. Int., 2024, 95: 2300674
[25] Li X L, Yang J W, Zhao L Y, et al. Solid solution strengthening type maraging stainless steel for low-temperature environment and preparation method of solid solution strengthening type maraging stainless steel [P]. Chin Pat, 202510074871.6, 2005
[25] 李小琳, 杨佳伟, 赵利媛 等. 一种低温环境用固溶强化型马氏体时效不锈钢及制备方法 [P]. 中国专利, 202510074871.6, 2025
[26] Gong P, Wynne B P, Knowles A J, et al. Effect of ageing on the microstructural evolution in a new design of maraging steels with carbon [J]. Acta Mater., 2020, 196: 101
[27] Knowles A J, Gong P, Rahman K M, et al. Development of Ni-free Mn-stabilised maraging steels using Fe2SiTi precipitates [J]. Acta Mater., 2019, 174: 260
[28] Song Y Y, Li X Y, Rong L J, et al. The Influence of tempering temperature on the reversed austenite formation and tensile properties in Fe-13%Cr-4%Ni-Mo low carbon martensite stainless steels [J]. Mater. Sci. Eng., 2011, A528: 4075
[29] Hubáčková I J, Číhal D I V, Mazanec P I K. Two-stage tempering of steel 13%Cr6%Ni [J]. Mater. Sci. Eng. Technol., 1984, 15: 411
[30] Wang P. Effect of reversed austenite on mechanical and corrosion properties of 13Cr super martensitic stainless steel [D]. Beijing: University of Science & Technology Beijing, 2023
[30] 王 鹏. 逆变奥氏体对13Cr超级马氏体不锈钢力学和腐蚀性能的影响 [D]. 北京: 北京科技大学, 2023
[31] Sinha P P, Sivakumar D, Babu N S, et al. Austenite reversion in 18-Ni Co-free maraging steel [J]. Steel Res., 1995, 66: 490
[32] Hsiao C N, Chiou C S, Yang J R. Aging reactions in a 17-4 PH stainless steel [J]. Mater. Chem. Phys., 2002, 74: 134
[33] Calcagnotto M, Ponge D, Demir E, et al. Orientation gradients and geometrically necessary dislocations in ultrafine grained dual-phase steels studied by 2D and 3D EBSD [J]. Mater. Sci. Eng., 2010, A527: 2738
[34] Hwang J K, Kim S J. Effect of reduction in area per pass on strain distribution and microstructure during caliber rolling in twinning-induced plasticity steel [J]. J. Iron Steel Res. Int., 2020, 27: 62
[35] Liu L X, Zhao L Y, Sun M, et al. Importance of cold rolling and tempering on the microstructure evolution, precipitation behavior and mechanical responses of 9Cr3Co3W1Cu ferritic/martensitic steel [J]. Mater. Charact., 2023, 206: 113376
[36] Sinha P P, Tharian K T, Sreekumar K, et al. Effect of aging on microstructure and mechanical properties of cobalt free 18%Ni (250 Grade) maraging steel [J]. Mater. Sci. Technol., 1998, 14: 1
[37] Liu C C, Yao K F, Liu Z, et al. Study of the effects of stress and strain on martensite transformation: Kinetics and transformation plasticity [J]. J. Comput. Aided Mater. Des., 2000, 7: 63
[38] Meyrick G, Powell G W. Phase transformations in metals and alloys [J]. Annu. Rev. Mater. Sci., 1973, 3: 327
[39] Chen X X, Guan L, Li W J, et al. Comparative study of corrosion rates determined by several methods for Q235 steel [J]. Mater. Prot., 2021, 54: 34
[39] 陈心欣, 关 蕾, 李万江 等. 表征Q235钢腐蚀速率的几种方法的比较研究 [J]. 材料保护, 2021, 54: 34
[40] Pu N, Chen J, Yin C J, et al. Investigation on pitting corrosion behavior of ultrafine-grained 304L stainless steel in Cl- containing solution [J]. Acta Metall. Sin., 2015, 51: 1077
[40] 朴 楠, 陈 吉, 尹成江 等. 超细晶304L不锈钢在含Cl-溶液中点蚀行为的研究 [J]. 金属学报, 2015, 51: 1077
[41] Deng B, Jiang Y M, Gong J, et al. Critical pitting and repassivation temperatures for duplex stainless steel in chloride solutions [J]. Electrochim. Acta, 2008, 53: 5220
[42] Yang J W, Tian L, Yang L, et al. Research on the corrosion resistance of hydraulic bracket cylinder barrel materials [J]. Found. Technol., 2024, 45: 342
[42] 杨佳伟, 田 雷, 杨 磊 等. 液压支架缸筒材料的耐蚀性研究 [J]. 铸造技术, 2024, 45: 342
[43] Olsson C O A, Landolt D. Passive films on stainless steels-chemistry, structure and growth [J]. Electrochim. Acta, 2003, 48: 1093
[44] He X, Lü X Y, Wu Z W, et al. M23C6 precipitation and Si segregation promoted by deep cryogenic treatment aggravating pitting corrosion of supermartensitic stainless steel [J]. J. Iron Steel Res. Int., 2021, 28: 629
[45] Martin F A, Bataillon C, Cousty J. In situ AFM detection of pit onset location on a 304L stainless steel [J]. Corros. Sci., 2007, 50: 84
[46] Balyanov A, Kutnyakova J, Amirkhanova N A, et al. Corrosion resistance of ultra fine-grained Ti [J]. Scr. Mater., 2004, 51: 225
[47] Wang W, Song S Z, Wang J F. The effect of heat treatment on the passive property of maraging stainless steel [J]. J. Chin. Soc. Corros. Protect., 1989, 9: 220
[47] 王 为, 宋诗哲, 王津凤. 热处理对马氏体时效不锈钢钝化特牲的影响 [J]. 中国腐蚀与防护学报, 1989, 9: 220
[48] Xue L, Ding Y, Pradeep K G, et al. The grain size effect on corrosion property of Al2Cr5Cu5Fe53Ni35 high-entropy alloy in marine environment [J]. Corros. Sci., 2022, 208: 110625
[49] Bommersbach P, Alemany-Dumont C, Millet J P, et al. Formation and behaviour study of an environment-friendly corrosion inhibitor by electrochemical methods [J]. Electrochim. Acta, 2005, 51: 1076
[50] Huang C X, Wang Y F, Ma X L, et al. Interface affected zone for optimal strength and ductility in heterogeneous laminate [J]. Mater. Today, 2018, 21: 713
[51] Hirschorn B, Orazem M E, Tribollet B, et al. Determination of effective capacitance and film thickness from constant-phase-element parameters [J]. Electrochim. Acta, 2010, 55: 6218
[1] 宋逸思, 廖瑜, 李传维, 陈益华, 顾剑锋. 逆转变奥氏体对0Cr16Ni5Mo1超级马氏体不锈钢低温冲击韧性的影响[J]. 金属学报, 2025, 61(5): 687-698.
[2] 袁涛, 赵晓虎, 蒋晓青, 任学磊, 李博阳. 脉冲电流辅助等离子弧焊Al-Mg合金晶粒细化机理[J]. 金属学报, 2024, 60(3): 323-332.
[3] 刘勇, 曾刚, 刘洪, 王煜, 李建龙. 含Zr镁合金晶粒细化机理与研究进展[J]. 金属学报, 2024, 60(2): 129-142.
[4] 王滨, 牛梦超, 王威, 姜涛, 栾军华, 杨柯. 含Cu马氏体时效不锈钢的组织与强韧性[J]. 金属学报, 2023, 59(5): 636-646.
[5] 李小兵, 潜坤, 舒磊, 张孟殊, 张金虎, 陈波, 刘奎. W含量对Ti-42Al-5Mn-xW合金相转变行为的影响[J]. 金属学报, 2023, 59(10): 1401-1410.
[6] 吴国华, 童鑫, 蒋锐, 丁文江. 铸造Mg-RE合金晶粒细化行为研究现状与展望[J]. 金属学报, 2022, 58(4): 385-399.
[7] 丁宁, 王云峰, 刘轲, 朱训明, 李淑波, 杜文博. 高应变速率多向锻造Mg-8Gd-1Er-0.5Zr合金的微观组织、织构及力学性能[J]. 金属学报, 2021, 57(8): 1000-1008.
[8] 刘振宝,梁剑雄,苏杰,王晓辉,孙永庆,王长军,杨志勇. 高强度不锈钢的研究及发展现状[J]. 金属学报, 2020, 56(4): 549-557.
[9] 李秀程,孙明煜,赵靖霄,王学林,尚成嘉. 铁素体-贝氏体/马氏体双相钢中界面的定量化晶体学表征[J]. 金属学报, 2020, 56(4): 653-660.
[10] 武华健, 程仁山, 李景仁, 谢东升, 宋锴, 潘虎成, 秦高梧. Al含量对Mg-Sn-Ca合金微观组织与力学性能的影响[J]. 金属学报, 2020, 56(10): 1423-1432.
[11] 张军,介子奇,黄太文,杨文超,刘林,傅恒志. 镍基铸造高温合金等轴晶凝固成形技术的研究和进展[J]. 金属学报, 2019, 55(9): 1145-1159.
[12] 邓丽萍,崔凯旋,汪炳叔,向红亮,李强. AZ31镁合金室温多道次压缩过程微观组织和织构演变的研究[J]. 金属学报, 2019, 55(8): 976-986.
[13] 李淑波, 杜文博, 王旭东, 刘轲, 王朝辉. Zr对Mg-Gd-Er合金晶粒细化机理的影响[J]. 金属学报, 2018, 54(6): 911-917.
[14] 杨柯, 牛梦超, 田家龙, 王威. 新一代飞机起落架用马氏体时效不锈钢的研究[J]. 金属学报, 2018, 54(11): 1567-1585.
[15] 毛轶哲, 李建国, 封蕾. 573 K高温时效处理的Al-10Mg合金中粗大β(Al3Mg2)相对热压缩组织演化的影响及机理[J]. 金属学报, 2018, 54(10): 1451-1460.