Please wait a minute...
金属学报  2025, Vol. 61 Issue (11): 1703-1714    DOI: 10.11900/0412.1961.2024.00086
  研究论文 本期目录 | 过刊浏览 |
选区激光熔化Ni58Cr23Fe10W5Ti2Ta1Nb1 多主元合金的裂纹形成机理及抑制
林美, 郭博静, 王志军, 李俊杰, 王雷, 王锦程, 何峰()
西北工业大学 凝固技术全国重点实验室 西安 710072
Crack Mechanism and Control Strategy for Ni58Cr23Fe10W5-Ti2Ta1Nb1 Multi-Principal Element Alloy by Selective Laser Melting
LIN Mei, GUO Bojing, WANG Zhijun, LI Junjie, WANG Lei, WANG Jincheng, HE Feng()
State Key Laboratory of Solidification Processing, Northwestern Polytechnical University, Xi'an 710072, China
引用本文:

林美, 郭博静, 王志军, 李俊杰, 王雷, 王锦程, 何峰. 选区激光熔化Ni58Cr23Fe10W5Ti2Ta1Nb1 多主元合金的裂纹形成机理及抑制[J]. 金属学报, 2025, 61(11): 1703-1714.
Mei LIN, Bojing GUO, Zhijun WANG, Junjie LI, Lei WANG, Jincheng WANG, Feng HE. Crack Mechanism and Control Strategy for Ni58Cr23Fe10W5-Ti2Ta1Nb1 Multi-Principal Element Alloy by Selective Laser Melting[J]. Acta Metall Sin, 2025, 61(11): 1703-1714.

全文: PDF(4311 KB)   HTML
摘要: 

利用选区激光熔化技术制备析出强化型高性能多主元合金存在难以成形的问题,极易开裂。本工作通过选区激光熔化制备Ni58Cr23Fe10W5Ti2Ta1Nb1 (含0.02%B,质量分数)多主元合金,揭示其裂纹形成机理,探索抑制裂纹形成的途径。结果表明,裂纹沿粗大柱状晶的晶界开裂,且优先出现在大角度晶界处,裂纹表面呈现光滑、清晰的树枝晶形貌,为典型的凝固裂纹。形成凝固裂纹的主要原因是:在凝固末期,B元素偏析于晶界,促进低熔点液膜产生,大角度晶界使得液膜保持稳定状态,循环加热/冷却导致的残余应力作用于液膜进而触发凝固开裂。热输入与开裂敏感性并非线性关系,仅通过调控热输入无法消除裂纹,只能在一定程度上抑制裂纹。通过添加TiB2纳米颗粒,增加晶界密度,缓解局部应力集中,成功消除了凝固裂纹。

关键词 : 选区激光熔化,  凝固裂纹,  开裂机理,  高熵合金    
Abstract:

With the increasing sophistication of laser additive manufacturing technology, the need for high-performance alloys suitable for additive manufacturing has grown. Developing new alloys with excellent mechanical properties and good formability has become a critical direction in the field of additive manufacturing, but severe defect-like cracking remains a major concern. Based on a new design concept from the corners of the phase diagrams to the central region, multi-principal element alloys (MPEAs, i.e., high-entropy alloys) have introduced new opportunities for the development of high-performance additive manufactured alloys. Ni58Cr23Fe10W5Ti2Ta1Nb1 MPEA (containing 0.02%B element, mass fraction) shows great potential for overcoming the severe trade-off between manufacturability and high strength. On the one hand, Ni58Cr23Fe10W5Ti2Ta1Nb1 MPEA has a yield strength of ~1 GPa and an elongation of ~25%, thus its comprehensive performance is superior to that of most existing MPEAs. On the other hand, because of its slower precipitation kinetics than the IN718 alloy, the main strengthening phase (γ″) of MPEA is stable at 800 oC, and thus it shows promise for eliminating the cracking of the precipitation-strengthened alloys. However, because Ni58Cr23Fe10W5Ti2Ta1Nb1 MPEA is a newly designed alloy, the effects of multi-principal alloying on its non-equilibrium solidification behavior are unknown, as is the mechanism of this effect, and its cracking behavior under additive manufacturing and corresponding mechanism must be evaluated. This work takes Ni58Cr23Fe10W5Ti2Ta1Nb1 MPEA as the research object and uses selective laser melting (SLM) technology and advanced characterization techniques to investigate the crack formation mechanism and control path of the alloy under different SLM process parameters. The formability of Ni58Cr23Fe10W5Ti2Ta1Nb1 alloy under different SLM process parameters was investigated, and the crack formation mechanism of Ni58Cr23Fe10W5Ti2Ta1Nb1 alloy was revealed. The crack control method was then explored. The results showed that the cracks propagated along the grain boundary of the coarse columnar crystals and preferentially appeared at high-angle grain boundaries (HAGBs). The surface of the cracks presented a smooth and clear dendritic morphology, which is a typical solidification crack. At the terminal stage of solidification, the HAGB regions contain a thin layer of B segregation, which promoted the production of a continuous liquid film, and the liquid film remained stable at HAGB owing to the large grain boundary energy. The residual stress caused by heating/cooling circulation acted on the liquid film and triggered solidification cracking. The relationship between the heat input and the cracking sensitivity was not linear. Cracks cannot be eliminated by simply regulating heat input, and cracks can be suppressed only to a certain extent. The grain boundary density increased, local stress concentration was alleviated, and solidification cracks were successfully eliminated with the addition of TiB2 nanoparticles.

Key words: selective laser melting    solidification crack    cracking mechanism    high-entropy alloy
收稿日期: 2024-03-18     
ZTFLH:  TG146  
基金资助:国家自然科学基金项目(52001266);中央高校基本科研业务费项目(G2022KY05109);广东省基础与应用基础研究基金项目(2023A1515012703);上海市“曙光”计划项目(23YF1450900);西北工业大学研究生实践创新基金项目(PF2023073)
通讯作者: 何 峰,fenghe1991@nwpu.edu.cn,主要从事高熵合金非平衡凝固加工及应用研究
Corresponding author: HE Feng, professor, Tel: 18710790457, E-mail: fenghe1991@nwpu.edu.cn
作者简介: 林 美,女,1999年生,硕士
图1  等离子旋转电极雾化制备Ni58Cr23Fe10W5Ti2Ta1Nb1多主元合金粉末的形貌、尺寸分布及EDS元素面扫描图
图2  TiB2纳米颗粒及1%TiB2纳米颗粒和Ni58Cr23Fe10W5Ti2Ta1Nb1合金粉末机械混合后的粉末形貌及EDS元素面扫描图
SampleCrFeWTiTaNbBCONi

Designed composition of powder

Practical composition of powder

18.7408.75211.5302.1312.8361.4560.360--Bal.
18.6008.89011.4002.0403.5001.6100.3100.0010.140Bal.
Practical composition of SLMed block19.0008.96010.5002.1603.3401.5900.2100.0590.078Bal.
表1  复合合金粉末及选区激光熔化成形块体的理论成分和实际成分 (mass fraction / %)
图3  67°逐层旋转的扫描策略
图4  不同工艺参数下选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金缺陷的OM像
图5  工艺参数对选区激光熔化成形Ni58Cr23Fe10W5Ti2-Ta1Nb1合金开裂行为的影响
图6  选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金在体能量密度Ev = 182.3 J/mm3 (激光功率P = 350 W、扫描速率v = 600 mm/s)下的裂纹分布特征
图7  不同体能量密度下选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金裂纹表面形貌的SEM像
图8  基于平衡凝固和Scheil型凝固路径的Ni58Cr23-Fe10W5Ti2Ta1Nb1合金热力学计算
图9  Ni58Cr23Fe10W5Ti2Ta1Nb1合金非平衡凝固过程中元素含量的变化曲线
图10  选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金裂纹附近的SEM像和EDS元素面扫描图
图11  选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金在Ev = 182.3 J/mm3下的应力分布特征
图12  体能量密度(热输入)对选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金开裂行为的影响
图13  在相同成形工艺参数下(P = 280 W、v = 1000 mm/s、层厚t = 0.04 mm、道间距h = 0.07 mm)选区激光熔化成形Ni58Cr23Fe10W5Ti2Ta1Nb1合金添加1%TiB2纳米颗粒前后的凝固组织
图14  在P = 280 W、v = 1000 mm/s、t = 0.04 mm、h = 0.07 mm成形工艺下TiB2改性Ni58Cr23Fe10W5Ti2-Ta1Nb1合金的熔池形貌
[1] Rometsch P A, Zhu Y M, Wu X H, et al. Review of high-strength aluminium alloys for additive manufacturing by laser powder bed fusion [J]. Mater. Des., 2022, 219: 110779
[2] Zhou W Z, Tian Y S, Tan Q B, et al. Effect of carbon content on the microstructure, tensile properties and cracking susceptibility of IN738 superalloy processed by laser powder bed fusion [J]. Addit. Manuf., 2022, 58: 103016
[3] Tang Y T, Panwisawas C, Ghoussoub J N, et al. Alloys-by-design: Application to new superalloys for additive manufacturing [J]. Acta Mater., 2021, 202: 417
[4] Stopyra W, Gruber K, Smolina I, et al. Laser powder bed fusion of AA7075 alloy: Influence of process parameters on porosity and hot cracking [J]. Addit. Manuf., 2020, 35: 101270
[5] Qi Z, Wang B, Zhang P, et al. Effects of stress ratio on the fatigue crack growth rate under steady state of selective laser melted TC4 alloy with defects [J]. Acta Metall. Sin., 2023, 59: 1411
[5] 戚 钊, 王 斌, 张 鹏 等. 应力比对含缺陷选区激光熔化TC4合金稳态疲劳裂纹扩展速率的影响 [J]. 金属学报, 2023, 59: 1411
[6] Wan H Y, Liu Z Z, Han Q Q, et al. Laser additive manufacturing of cracking-resistant superalloys [J]. Aeronaut. Sci. Technol., 2022, 33: 26
[6] 万宏远, 刘壮壮, 韩泉泉 等. 激光增材制造高温合金抗开裂行为研究进展 [J]. 航空科学技术, 2022, 33: 26
[7] Zhu G L, Kong D C, Zhou W Z, et al. Research progress on the crack formation mechanism and cracking-free design of γ' phase strengthened nickel-based superalloys fabricated by selective laser melting [J]. Acta Metall. Sin., 2023, 59: 16
[7] 祝国梁, 孔德成, 周文哲 等. 选区激光熔化γ'相强化镍基高温合金裂纹形成机理与抗裂纹设计研究进展 [J]. 金属学报, 2023, 59: 16
[8] Chandra S, Tan X P, Narayan R L, et al. A generalised hot cracking criterion for nickel-based superalloys additively manufactured by electron beam melting [J]. Addit. Manuf., 2021, 37: 101633
[9] Zhou Z P, Huang L, Shang Y J, et al. Causes analysis on cracks in nickel-based single crystal superalloy fabricated by laser powder deposition additive manufacturing [J]. Mater. Des., 2018, 160: 1238
[10] Chauvet E, Kontis P, Jägle E A, et al. Hot cracking mechanism affecting a non-weldable Ni-based superalloy produced by selective electron beam melting [J]. Acta Mater., 2018, 142: 82
[11] Sun Z J, Ma Y, Ponge D, et al. Thermodynamics-guided alloy and process design for additive manufacturing [J]. Nat. Commun., 2022, 13: 4361
[12] Wu S W, Chia H Y, Zhang T L, et al. A precipitation strengthened high entropy alloy with high (Al + Ti) content for laser powder bed fusion: Synergizing in trinsic hot cracking resistance and ultrahigh strength [J]. Acta Mater., 2023, 258: 119193
[13] Guo C, Li G, Zhou F, et al. Understanding the significant effect of boron content on the printability of IN738LC superalloy fabricated using laser powder bed fusion [J]. Opt. Laser Technol., 2023, 159: 108954
[14] Lv Y T, Zhang Z, Zhang Q, et al. Cracking inhibition behavior and the strengthening effect of TiC particles on the CM247LC superalloy prepared by selective laser melting [J]. Mater. Sci. Eng., 2022, A858: 144119
[15] Zhang Z H, Han Q Q, Yang S Z, et al. Laser powder bed fusion of advanced submicrometer TiB2 reinforced high-performance Ni-based composite [J]. Mater. Sci. Eng., 2021, A817: 141416
[16] Zhao Y N, Ma Z Q, Yu L M, et al. New alloy design approach to inhibiting hot cracking in laser additive manufactured nickel-based superalloys [J]. Acta Mater., 2023, 247: 118736
[17] Adegoke O, Andersson J, Brodin H, et al. Influence of laser powder bed fusion process parameters on the microstructure and cracking susceptibility of nickel-based superalloy alloy 247LC [J]. Results Mater., 2022, 13: 100256
[18] Liu L Q, Wang D, Deng G W, et al. Crack inhibition to enhance strength-ductility of CM247LC alloy fabricated by laser powder bed fusion [J]. Mater. Sci. Eng., 2023, A875: 145114
[19] Kontis P, Chauvet E, Peng Z R, et al. Atomic-scale grain boundary engineering to overcome hot-cracking in additively-manufactured superalloys [J]. Acta Mater., 2019, 177: 209
[20] Jeong S G, Ahn S Y, Kim E S, et al. Liquation cracking in laser powder bed fusion-fabricated Inconel718 of as-built, stress-relieved, and hot isostatic pressed conditions [J]. Mater. Sci. Eng., 2023, A888: 145797
[21] Xu J J, Lin X, Zhao Y F, et al. HAZ liquation cracking mechanism of IN-738LC superalloy prepared by laser solid forming [J]. Metall. Mater. Trans., 2018, 49: 5118
[22] Barker J F. The initial years of Alloy 718—A GE perspective [J]. Superalloy, 1989, 718: 269
[23] Lin M, Lu J L, Chen Y M, et al. 800 oC-stable D022 superlattice in a NiCrFe-based medium entropy alloy [J]. Mater. Res. Lett., 2024, 12: 172
[24] Harrison N J, Todd I, Mumtaz K. Reduction of micro-cracking in nickel superalloys processed by selective laser melting: A fundamental alloy design approach [J]. Acta Mater., 2015, 94: 59
[25] Liu X X, Hu R, Luo X, et al. A high-strength Ni-Cr-W based superalloy prepared by laser powder bed fusion: Printability, microstructure and tensile properties [J]. Mater. Sci. Eng., 2022, A853: 143744
[26] Yang X G, Zhou Y, Xi S Q, et al. Additively manufactured fine grained Ni6Cr4WFe9Ti high entropy alloys with high strength and ductility [J]. Mater. Sci. Eng., 2019, A767: 138394
[27] Han Q Q, Gu Y C, Setchi R, et al. Additive manufacturing of high-strength crack-free Ni-based Hastelloy X superalloy [J]. Addit. Manuf., 2019, 30: 100919
[28] Sun Z, Tan X P, Descoins M, et al. Revealing hot tearing mechanism for an additively manufactured high-entropy alloy via selective laser melting [J]. Scr. Mater., 2019, 168: 129
[29] Niu P D, Li R D, Fan Z Q, et al. Inhibiting cracking and improving strength for additive manufactured Al x CoCrFeNi high entropy alloy via changing crystal structure from BCC-to-FCC [J]. Addit. Manuf., 2023, 71: 103584
[30] Li R D, Niu P D, Yuan T C, et al. Selective laser melting of an equiatomic CoCrFeMnNi high-entropy alloy: Processability, non-equilibrium microstructure and mechanical property [J]. J. Alloys Compd., 2018, 746: 125
[31] Song C H, Fu H X, Yan Z W, et al. Internal defects and control methods of laser powder bed fusion forming [J]. Chin. J. Lasers, 2022, 49: 1402801
[31] 宋长辉, 付厚雄, 严仲伟 等. 激光粉末床熔融成形内部质量缺陷及其调控方法 [J]. 中国激光, 2022, 49: 1402801
[32] Chuang P Y, Huang M J. Model and simulation predictions of the thermal conductivity of compact random nanoparticle composites [J]. Int. J. Heat Mass Tranfer, 2013, 61: 490
[33] Rappaz M, Jacot A, Boettinger W J. Last-stage solidification of alloys: Theoretical model of dendrite-arm and grain coalescence [J]. Metall. Mater. Trans., 2003, 34A: 467
[34] Zhang J, Singer R F. Hot tearing of nickel-based superalloys during directional solidification [J]. Acta Mater., 2002, 50: 1869
[35] Dai K, Shaw L. Thermal and mechanical finite element modeling of laser forming from metal and ceramic powders [J]. Acta Mater., 2004, 52: 69
[36] Gu D D, Yuan P P. Thermal evolution behavior and fluid dynamics during laser additive manufacturing of Al-based nanocomposites: underlying role of reinforcement weight fraction [J]. J. Appl. Phys., 2015, 118: 233109
[37] Li X P, Ji G, Chen Z, et al. Selective laser melting of nano-TiB2 decorated AlSi10Mg alloy with high fracture strength and ductility [J]. Acta Mater., 2017, 129: 183
[38] Ma C, Zhao J Z, Cao C Z, et al. Fundamental study on Laser interactions with nanoparticles-reinforced metals—Part I: Effect of nanoparticles on optical reflectivity, specific heat, and thermal conductivity [J]. J. Manuf. Sci. Eng., 2016, 138: 121001
[39] Nan C W, Birringer R, Clarke D R, et al. Effective thermal conductivity of particulate composites with interfacial thermal resistance [J]. J. Appl. Phys., 1997, 81: 6692
[40] Ordonez-Miranda J, Alvarado-Gil J J. Thermal conductivity of nanocomposites with high volume fractions of particles [J]. Compos. Sci. Technol., 2012, 72: 853
[41] DebRoy T, Wei H L, Zuback J S, et al. Additive manufacturing of metallic components—Process, structure and properties [J]. Prog. Mater. Sci., 2018, 92: 112
[42] Chen Z, Wen X L, Wang W L, et al. Engineering fine grains, dislocations and precipitates for enhancing the strength of TiB2-modified CoCrFeMnNi high-entropy alloy using laser powder bed fusion [J]. J. Mater. Res. Technol., 2023, 26: 1198
[43] Zhang Z H, Han Q Q, Liu Z Y, et al. Influence of the TiB2 content on the processability, microstructure and high-temperature tensile performance of a Ni-based superalloy by laser powder bed fusion [J]. J. Alloys Compd., 2022, 908: 164656
[44] Zhang Z H, Han Q Q, Liu Z Y, et al. Cracking behaviour and its suppression mechanisms with TiB2 additions in the laser additive manufacturing of solid-solution-strengthened Ni-based alloys [J]. Composites, 2023, 266B: 111023
[45] Zhang C, Zhu J K, Zhang G Q, et al. Laser powder bed fusion of nano-TiB2 reinforced FeCoNiCr high-entropy alloy with enhanced strength and firm corrosion resistance [J]. J. Alloys Compd., 2022, 927: 167110
[46] Zhao M Q, Song J, Tang Q, et al. Laser powder bed fusion of Inconel 718-based composites: Effect of TiB2 content on microstructure and mechanical performance [J]. Opt. Laser Technol., 2023, 167: 109596
[47] Zhang J, Singer R F. Effect of grain-boundary characteristics on castability of nickel-base superalloys [J]. Metall. Mater. Trans., 2004, 35A: 939
[48] Zhou Y Z, Volek A. Effect of grain boundary fraction on castability of a directionally solidified nickel alloy [J]. Scr. Mater., 2006, 54: 2169
[49] Hoffman A K, Zhang Y F, Arivu M, et al. Novel effects of grain size and ion implantation on grain boundary segregation in ion irradiated austenitic steel [J]. Acta Mater., 2023, 246: 118714
[50] Zhou W Z, Zhu G L, Wang R, et al. Inhibition of cracking by grain boundary modification in a non-weldable nickel-based superalloy processed by laser powder bed fusion [J]. Mater. Sci. Eng., 2020, A791: 139745
[51] Sun Z J, Sun B H, Soh V, et al. Laser powder bed fusion of crack-susceptible stainless maraging steel undergoing solid-state phase transformations [J]. Acta Mater., 2024, 263: 119534
[52] Wang S Y, Wu Y X, He F. Review of the heterogeneous microstructures, precipitation behavior and mechanical properties of additively manufactured precipitation-strengthened high-entropy alloys [J]. Foundry Technol., 2025, 46: 774
[52] 王松宇, 吴宜霞, 何 峰. 增材制造析出强化型高熵合金非均匀组织、析出行为及力学性能研究进展 [J]. 铸造技术, 2025, 46: 774
[53] Chen C Y, Wang J, Wang R X, et al. Research progress and prospect of additive manufacturing of key materials for aeroengines and gas turbines [J]. Sci. Technol. Rev., 2023, 41(5): 34
[53] 陈超越, 王 江, 王瑞鑫 等. 航空发动机及燃气轮机用关键材料的激光增材制造研究进展 [J]. 科技导报, 2023, 41(5): 34
[1] 雷云龙, 杨康, 辛越, 姜自滔, 童宝宏, 张世宏. 机械合金化AlCrCu0.5Mo0.5Ni高熵合金及其后续退火态的结构演化[J]. 金属学报, 2025, 61(5): 731-743.
[2] 王家骏, 袁野, 何竹风, 朱明伟, 贾楠. 基于轧制温度调控的Fe50Mn29Co10Cr10Cu1 高熵合金微观组织与力学性能[J]. 金属学报, 2025, 61(10): 1502-1514.
[3] 王志军, 白晓昱, 王健斌, 姜慧, 焦文娜, 李天昕, 卢一平. 共晶高熵合金十年发展回顾(2014—2024):设计、制备与应用[J]. 金属学报, 2025, 61(1): 1-11.
[4] 夏兴川, 张恩宽, 丁俭, 王玉江, 刘永长. 激光熔覆难熔高熵合金涂层研究进展[J]. 金属学报, 2025, 61(1): 59-76.
[5] 朱满, 张成, 许军锋, 坚增运, 惠增哲. CrNbTiVAl x 难熔高熵合金的组织、力学性能和高温氧化行为[J]. 金属学报, 2025, 61(1): 88-98.
[6] 王叶青, 付珂, 赵永柱, 苏礼季, 陈正. Fe7(CoNiMn)80B13 共晶高熵合金的深过冷非平衡凝固行为及微观组织演变[J]. 金属学报, 2025, 61(1): 143-153.
[7] 韩英, 吴雨航, 赵春禄, 张靖实, 李振民, 冉旭. 选区激光熔化成形Al-Si-Fe-Mn-Ni合金的高温蠕变行为[J]. 金属学报, 2025, 61(1): 154-164.
[8] 卢健麟, 任化永, 谢桉, 王建潼, 何峰. Ni43.5Co19Cr10Fe10Al15Ti2Mo0.5 共晶高熵合金快速凝固行为及组织调控[J]. 金属学报, 2025, 61(1): 191-202.
[9] 王瀚铭, 杜银, 裴旭辉, 王海丰. 共晶组织强化NbMoZrVSi x 难熔高熵合金的摩擦磨损性能及磨损机理[J]. 金属学报, 2024, 60(7): 937-946.
[10] 蔡宣明, 张伟, 范志强, 高玉波, 王俊元, 张柱军. AlSi10Mg多孔结构在不同加载应变率下的损伤模式及响应机制[J]. 金属学报, 2024, 60(7): 857-868.
[11] 张楠, 张海武, 王淼辉. 微米级选区激光熔化316L不锈钢的拉伸力学性能[J]. 金属学报, 2024, 60(2): 211-219.
[12] 唐旭, 张昊, 薛鹏, 吴利辉, 刘峰超, 朱正旺, 倪丁瑞, 肖伯律, 马宗义. 铸态及激光粉末床熔融AlCoCrFeNi2.1 共晶高熵合金的微观组织及力学性能[J]. 金属学报, 2024, 60(11): 1461-1470.
[13] 张振武, 李继康, 许文贺, 沈沐宇, 戚磊一, 郑可盈, 李伟, 魏青松. 搭接工艺对选区激光熔化镍基单晶高温合金DD491晶体取向与微观组织的影响[J]. 金属学报, 2024, 60(11): 1471-1486.
[14] 陈玉勇, 时国浩, 杜之明, 张宇, 常帅. 增材制造TiAl合金的研究进展[J]. 金属学报, 2024, 60(1): 1-15.
[15] 张海峰, 闫海乐, 方烽, 贾楠. FeMnCoCrNi高熵合金双晶微柱变形机制的分子动力学模拟[J]. 金属学报, 2023, 59(8): 1051-1064.