高熵稀土单硅酸盐环境障涂层局域结构的原子对分布函数解析
王浩宇1, 吕熙睿1, 陈琦1,2, 熊瑛3, 罗志新1, 张洁1(), 王京阳1
1 中国科学院金属研究所 沈阳材料科学国家实验室 沈阳 110016
2 中国科学技术大学 材料科学与工程学院 合肥 230000
3 中国航发沈阳黎明航空发动机有限责任公司 沈阳 110043
Neutron Pair Distribution Function Analysis to the Local Structure of High-Entropy RE2SiO5 Environmental Barrier Coating
WANG Haoyu1, LÜ Xirui1, CHEN Qi1,2, XIONG Ying3, LUO Zhixin1, ZHANG Jie1(), WANG Jingyang1
1 Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
2 School of Materials Science and Engineering, University of Science and Technology of China, Hefei 230000, China
3 AECC Shenyang Liming AERO-ENGINE Science and Technology Co. Ltd., Shenyang 110043, China
引用本文:

王浩宇, 吕熙睿, 陈琦, 熊瑛, 罗志新, 张洁, 王京阳. 高熵稀土单硅酸盐环境障涂层局域结构的原子对分布函数解析[J]. 金属学报, 2024, 60(8): 1130-1140.
Haoyu WANG, Xirui LÜ, Qi CHEN, Ying XIONG, Zhixin LUO, Jie ZHANG, Jingyang WANG. Neutron Pair Distribution Function Analysis to the Local Structure of High-Entropy RE2SiO5 Environmental Barrier Coating[J]. Acta Metall Sin, 2024, 60(8): 1130-1140.

全文: PDF(2562 KB)   HTML
摘要: 

调控稀土单硅酸盐(RE2SiO5)环境障涂层热膨胀系数,优化其与碳化硅纤维增强碳化硅(SiCf/SiC)陶瓷基复合材料基体热膨胀系数匹配性,是其应用于高推比航空发动机的关键。本工作基于RE2SiO5/Yb2Si2O7/Si三层结构涂层体系,对比研究了采用与基体热膨胀系数匹配优的(Y1/4Ho1/4Er1/4Yb1/4)2SiO5面层与典型Yb2SiO5面层涂层体系的抗热冲击性能,发现Yb2SiO5面层热膨胀系数偏大造成的应力累积,是导致三层结构涂层失效的主要原因。依据中子衍射数据,分析中子对分布函数,对2种单硅酸盐局域结构特征进行解析。结果表明,高熵稀土单硅酸盐中多种稀土元素协同作用,降低了[ORE4]四面体畸变程度,表现为热膨胀系数减小。提出通过合理选择稀土元素组合,扰动[ORE4]局域结构畸变,有望实现稀土单硅酸盐热膨胀系数的定向调控。

关键词 : 中子衍射,  原子对分布函数,  稀土硅酸盐,  环境障涂层,  燃气热冲击    
Abstract:

Environmental barrier coatings (EBCs) enable SiCf/SiC ceramic matrix composites (CMC) to operate under high-temperature combustion conditions. They reduce the oxidation rate of SiCf/SiC, the volatilization of the composites due to reaction with water vapor, and the surface temperature of the composites. Rare-earth monosilicates (RE2SiO5), owing to their excellent high-temperature durability, low thermal conductivity, and good phase stability, are used as the top layer of EBCs. However, they exhibit a high coefficient of thermal expansion (CTE), leading to thermal mismatch and inducing tensile residual stress (with a magnitude of several hundred MPa) in the coating, resulting in the formation of vertical cracks, which act as extremely-high-diffusivity paths for oxidation species transportation and silica volatilization. Therefore, regulating the CTE of RE2SiO5 EBCs and minimizing the CTE mismatch among constituent RE2SiO5 layers with SiCf/SiC CMCs are critical for multilayered EBCs. Through atmospheric plasma spraying, a typical Yb2SiO5/Yb2Si2O7/Si coating system and a tri-layer structured multicomponent (Y1/4Ho1/4Er1/4Yb1/4)2SiO5/Yb2Si2O7/Si coating system with better matched CTEs were manufactured. Both the coatings remained adhered to the substrate during deposition and after annealing, and no mud cracks that would compromise the coating gas-tightness quality and delamination cracks were observed at any of the coating interfaces. In thermal cycling tests, (Y1/4Ho1/4Er1/4Yb1/4)2SiO5/Yb2Si2O7/Si coatings showed a lifetime that is three times longer than that of conventional Yb2SiO5/Yb2Si2O7/Si coatings. The failure mechanisms in thermal cycling were investigated via the finite element simulation of stress. It was found that the stress in the substrate was low, and the residual thermal stress was mainly concentrated on the top, inter, and bond layers and increased with an increase in temperature. Compared with that of the (Y1/4Ho1/4Er1/4Yb1/4)2SiO5 top coat, the Yb2SiO5 top coat showed obviously higher residual tensile stress, which contributed to a higher tendency for mud-crack formation and higher energy release rate, substantially reducing the coating's thermal cycling lifetime. Through neutron powder diffraction and pair distribution function (PDF) analysis, the average and local structures of RE2SiO5 were studied. Overall, the average and local structures did not differ significantly, both of which can be described using the C2/c structure. Nevertheless, the PDF results demonstrated some differences in the disorder degree of Si—O and RE—O coordination environments. In particular, Rietveld refinement results of the PDF showed lower local distortion degree of [ORE4] tetrahedrons when compared with that of the average structure. It is effective to reduce the distortion degree of [ORE4] tetrahedrons by introducing Y3+, Ho3+, and Er3+ into the Yb3+ sites of Yb2SiO5, and smaller distortion degrees lead to lower CTE values. Coordinative local disturbances introduced by strategic high-entropy design have been proposed as the key method for CTE regulation.

Key words: neutron diffraction    pair distribution function    rare-earth silicate    environmental barrier coating    burner rig test
收稿日期: 2024-04-23     
ZTFLH:  TG174.4  
基金资助:国家自然科学基金项目(U21A2063);国家自然科学基金项目(52372071);国家自然科学基金项目(52302076);国家自然科学基金项目(92360304)
通讯作者: 张 洁,jiezhang@imr.ac.cn,主要从事极端环境陶瓷涂层应用基础研究
Corresponding author: ZHANG Jie, professor, Tel: (024)23970490, E-mail: jiezhang@imr.ac.cn
作者简介: 王浩宇,男,1994年生,博士
Coating

Current

A

Ar flow rate

L·min-1

H2 flow rate

L·min-1

Distance

mm

Si50042890
Yb2Si2O74504012120
Yb2SiO55504012120
(Y1/4Ho1/4Er1/4Yb1/4)2SiO55504012120
表1  RE2SiO5面层、Yb2Si2O7中间层及Si粘结层的制备参数
图1  三层结构环境障涂层(EBC)的SEM像及有限元网格模型
LayerMaterialYoung's modulus / GPaCTE / (106 K-1)Ref.
SubstrateSiC4304.02[25]
Bond layerSi82*4.10[23]
Inter layerYb2Si2O772-85*4.66[22,26]
Yb2SiO570-80*6.5-7.32[27]
Top layerYb2O390.85*6.07-8.03[28]
(4RE1/4)2SiO572.5-85*5.49-6.59[10]
表2  EBC各层的Young's模量及热膨胀系数(CTE)[10,22,23,25~29]
图2  (Y1/4Ho1/4Er1/4Yb1/4)2SiO5/Yb2Si2O7/Si和Yb2SiO5/Yb2Si2O7/Si涂层退火态XRD谱
CoatingPhase composition (mass fraction / %)Refinement factor / %
RE2SiO5RE2O3R-weighted pattern (Rwp)R-pattern (Rp)
(Y1/4Ho1/4Er1/4Yb1/4)2SiO576.323.74.943.65
Yb2SiO573.326.77.915.79
表3  (Y1/4Ho1/4Er1/4Yb1/4)2SiO5面层和Yb2SiO5面层Rietveld定量相分析结果及相应的精修因子
图3  (Y1/4Ho1/4Er1/4Yb1/4)2SiO5/Yb2Si2O7/Si和Yb2SiO5/Yb2Si2O7/Si涂层退火态与热循环后的SEM整体截面形貌及纵向裂纹放大形貌
图4  (Y1/4Ho1/4Er1/4Yb1/4)2SiO5/Yb2Si2O7/Si和Yb2SiO5/Yb2Si2O7/Si涂层由不同温度冷却到室温时各层残余热应力对比
图5  稀土单硅酸盐RE2SiO5的晶体结构示意图
图6  (Y1/4Ho1/4Er1/4Yb1/4)2SiO5和Yb2SiO5的飞行时间中子粉末衍射(TOF-NPD) Rietveld精修结果
Data sourceMaterialλσ2
[SiO4][ORE4][SiO4][ORE4]
TheoreticalYb2SiO51.000081.0014314.8653249.768
Average structure from TOFYb2SiO51.001341.0015614.21285.91
(Y1/4Ho1/4Er1/4Yb1/4)2SiO51.000061.0026022.99263.72
Local structure from PDFYb2SiO51.002741.0039158.25250.10
(Y1/4Ho1/4Er1/4Yb1/4)2SiO51.002131.0009975.00204.32
表4  Yb2SiO5与(Y1/4Ho1/4Er1/4Yb1/4)2SiO5的键长畸变度(λ)和键角畸变度(σ2)
图7  采用Rietveld精修TOF-NPD数据获得的RE2SiO5晶体结构直接拟合PDF的拟合结果
图8  (Y1/4Ho1/4Er1/4Yb1/4)2SiO5和Yb2SiO5的PDF谱图PDFgui精修结果及拟合结构的原子对分析
图9  Yb2SiO5和(Y1/4Ho1/4Er1/4Yb1/4)2SiO5在0.15~0.5 nm范围内的PDF谱图与精修结果
1 More K L, Tortorelli P F, Walker L R, et al. High-temperature stability of SiC-based composites in high-water-vapor-pressure environments [J]. J. Am. Ceram. Soc., 2003, 86: 1272
2 Zhang J, Liu R J, Jian Y J, et al. Degradation mechanism of SiCf/SiC composites after long-time water vapor and oxygen corrosion at 1300oC [J]. Corros. Sci., 2022, 197: 110099.
3 Tian Z L, Zhang J, Zheng L Y, et al. General trend on the phase stability and corrosion resistance of rare earth monosilicates to molten calcium-magnesium-aluminosilicate at 1300oC [J]. Corros. Sci., 2019, 148: 281
4 Sun L C, Ren X M, Du T F, et al. High entropy engineering: New strategy for the critical property optimizations of rare earth silicates [J]. J. Inorg. Mater., 2021, 36: 339
doi: 10.15541/jim20200611
4 孙鲁超, 任孝旻, 杜铁峰 等. 高熵化设计: 稀土硅酸盐材料关键性能优化新策略 [J]. 无机材料学报, 2021, 36: 339
doi: 10.15541/jim20200611
5 Lee K N. Current status of environmental barrier coatings for Si-based ceramics [J]. Surf. Coat. Technol., 2000, 133: 1
6 Luo Y X, Sun L C, Wang J M, et al. Tunable thermal properties in yttrium silicates switched by anharmonicity of low-frequency phonons [J]. J. Eur. Ceram. Soc., 2018, 38: 2043
7 Richards B T, Begley M R, Wadley H N G. Mechanisms of ytterbium monosilicate/mullite/silicon coating failure during thermal cycling in water vapor [J]. J. Am. Ceram. Soc., 2015, 98: 4066
8 Tian Z L, Zheng L Y, Hu W P, et al. Tunable properties of (Ho x Y1 - x )2SiO5 as damage self-monitoring environmental/thermal barrier coating candidates [J]. Sci. Rep., 2019, 9: 415
9 Cao G, Ouyang J H, Li Y, et al. Improved thermophysical properties of rare-earth monosilicates applied as environmental barrier coatings by adjusting structural distortion with RE-doping [J]. J. Eur. Ceram. Soc., 2021, 41: 7222
10 Ren X M, Tian Z L, Zhang J, et al. Equiatomic quaternary (Y1/4Ho1/4Er1/4Yb1/4)2SiO5 silicate: A perspective multifunctional thermal and environmental barrier coating material [J]. Scr. Mater., 2019, 168: 47
11 Li Y R, Wang J M, Wang J Y. Theoretical investigation of phonon contributions to thermal expansion coefficients for rare earth monosilicates RE2SiO5 (RE = Dy, Ho, Er, Tm, Yb and Lu) [J]. J. Eur. Ceram. Soc., 2020, 40: 2658
12 Luo Y X, Sun L C, Wang J M, et al. Material-genome perspective towards tunable thermal expansion of rare-earth di-silicates [J]. J. Eur. Ceram. Soc., 2018, 38: 3547
13 Hou D, Zhao C H, Paterson A R, et al. Local structures of perovskite dielectrics and ferroelectrics via pair distribution function analyses [J]. J. Eur. Ceram. Soc., 2018, 38: 971
14 Wei Z N. Design of lattice oxygen activity and local structural for lithium-rich layered oxide cathode material [D]. Xuzhou: China University of Mining and Technology, 2022
14 魏志宁. 富锂层状氧化物正极材料晶格氧活性及局域结构的设计 [D]. 徐州: 中国矿业大学, 2022
15 Ou M Y. Studies on the structure-properties relationship of disordered electrode materials by pair distribution function technique [D]. Wuhan: Huazhong University of Science and Technology, 2021
15 欧明洋. 原子对分布函数技术对无序电极材料构效关系的研究 [D]. 武汉: 华中科技大学, 2021
16 Xu Y, Ou M Y, Liu Y, et al. Crystallization-induced ultrafast naion diffusion in nickel hexacyanoferrate for high-performance sodium-ion batteries [J]. Nano Energy, 2020, 67: 104250
17 Li Z F, Chen Y C, Jian Z L, et al. Defective hard carbon anode for Na-ion batteries [J]. Chem. Mater., 2018, 30: 4536
18 Zhang N, Yokota H, Glazer A M, et al. The missing boundary in the phase diagram of PbZr1 - x Ti x O3 [J]. Nat. Commun., 2014, 5: 5231
doi: 10.1038/ncomms6231 pmid: 25342592
19 Datta K, Richter A, Göbbels M, et al. Direct mapping of microscopic polarization in ferroelectric x(BiScO3)-(1 - x)(PbTiO3) throu-ghout its morphotropic phase boundary [J]. Phys. Rev., 2016, 93B: 064102.
20 Mangelis P, Koch R J, Lei H, et al. Correlated disorder-to-order crossover in the local structure of K x Fe2 - y Se2 - z S z [J]. Phys. Rev., 2019, 100B: 094108
21 Campi G, Ricci A, Bianconi A. Local structure in Mg1 - x Al x B2 system by high resolution neutron diffraction [J]. J. Supercond. Nov. Magn., 2012, 25: 1319
22 Tian Z L, Zheng L Y, Wang J M, et al. Damage tolerance and extensive plastic deformation of β-Yb2Si2O7 from room to high temperatures [J]. J. Am. Ceram. Soc., 2015, 98: 2843
23 Richards B T, Sehr S, de Franqueville F, et al. Fracture mechanisms of ytterbium monosilicate environmental barrier coatings during cyclic thermal exposure [J]. Acta Mater., 2016, 103: 448
24 Wu S. Preparation and performance optimization of plasma sprayed Gd2O3-Yb2O3-YSZ composite thermal barrier coatings [D]. Shanghai: Shanghai Maritime University, 2022
24 吴 硕. 等离子喷涂Gd2O3-Yb2O3-YSZ复合热障涂层的制备及性能优化研究 [D]. 上海: 上海海事大学, 2022
25 Lee K N, Fox D S, Bansal N P. Rare earth silicate environmental barrier coatings for SiC/SiC composites and Si3N4 ceramics [J]. J. Eur. Ceram. Soc., 2005, 25: 1705
26 Zhou Y C, Zhao C, Wang F, et al. Theoretical prediction and experimental investigation on the thermal and mechanical properties of bulk β-Yb2Si2O7 [J]. J. Am. Ceram. Soc., 2013, 96: 3891
27 Tian Z L, Zheng L Y, Wang J M, et al. Theoretical and experimental determination of the major thermo-mechanical properties of RE2SiO5 (RE = Tb, Dy, Ho, Er, Tm, Yb, Lu, and Y) for environmental and thermal barrier coating applications [J]. J. Eur. Ceram. Soc., 2016, 36: 189
28 Zhang G H, Zhang J, Wang J Y. Synthesis and characterization of ytterbium oxide: A novel CMAS-resistant environmental barrier coating material [J]. J. Am. Ceram. Soc., 2023, 106: 621
29 Toby B H, von Dreele R B. GSAS-II: The genesis of a modern open-source all purpose crystallography software package [J]. J. Appl. Cryst., 2013, 46: 544
30 Richards B T, Zhao H B, Wadley H N G. Structure, composition, and defect control during plasma spray deposition of ytterbium silicate coatings [J]. J. Mater. Sci., 2015, 50: 7939
31 Li Y R. First-principles investigations about thermal properties of novel ceramics with low thermal conductivity [D]. Beijing: University of Chinese Academy of Sciences (Institute of Metal Research, Chinese Academy of Sciences), 2018
31 李亦然. 几种新型低热导率陶瓷热学性能的第一性原理研究 [D]. 北京: 中国科学院大学 (中国科学院金属研究所), 2018
32 Robinson K, Gibbs G V, Ribbe P H. Quadratic elongation: A quantitative measure of distortion in coordination polyhedra [J]. Science, 1971, 172: 567
pmid: 17802221
33 Zhu H, Huang Y L, Ren J C, et al. Bridging structural inhomogeneity to functionality: Pair distribution function methods for functional materials development [J]. Adv. Sci., 2021, 8: 2003534
34 Qiu X, Božin E S, Juhas P, et al. Reciprocal-space instrumental effects on the real-space neutron atomic pair distribution function [J]. J. Appl. Cryst., 2004, 37: 110
35 Lu Y H, Cao Y J, Zhao X. Optimal rare-earth disilicates as top coat in multilayer environmental barrier coatings [J]. J. Alloys Compd., 2018, 769: 1026
36 Wang Y W, Niu Y R, Zhong X, et al. Water vapor corrosion behaviors of plasma sprayed RE2SiO5 (RE = Gd, Y, Er) coatings [J]. Corros. Sci., 2020, 167: 108529
37 Jiang F R, Cheng L F, Wei H J, et al. Hot corrosion behavior of Lu2SiO5 and La2SiO5 in a molten Na2SO4 environment: A first-principles corrosion resistance investigation [J]. Ceram. Int., 2019, 45: 15532
[1] 周牧, 王倩, 王延绪, 翟梓融, 何伦华, 李昺, 马英杰, 雷家峰, 杨锐. 焊前预处理对钛合金厚板焊接残余应力的影响[J]. 金属学报, 2024, 60(8): 1064-1078.
[2] 任卫军, 安萌, 高飞, 罗小华, 李昺, 张志东, 王进威. 三方Cr5Te8 的磁结构和反常热膨胀[J]. 金属学报, 2024, 60(8): 1150-1154.
[3] 李彪, 张龙, 颜廷毅, 付华萌, 袁旭东, 文明月, 张宏伟, 李宏, 张海峰. 热处理工艺和W丝特性对W丝增强锆基非晶复合材料残余应力的影响[J]. 金属学报, 2024, 60(8): 1055-1063.
[4] 林皓, 李建, 杨钊龙, 钟圣怡. 中子衍射应力分析技术及其应用进展[J]. 金属学报, 2024, 60(8): 1017-1030.
[5] 朱桂杰, 王思清, 查敏, 李眉娟, 孙凯, 陈东风. 稀土元素Ce对挤压态Mg-0.3Al-0.2Ca-0.5Mn合金板材体织构及力学各向异性的影响[J]. 金属学报, 2024, 60(8): 1079-1090.
[6] 谷黎明, 冯效铭, 于朝, 张峻凡, 刘振宇, 何伦华, 卢怀乐, 李小虎, 王晨, 张晓东, 肖伯律, 马宗义. 深冷循环对SiC/Al复合材料宏微观残余应力的影响[J]. 金属学报, 2024, 60(8): 1031-1042.
[7] 杨俊杰, 张昌盛, 李洪佳, 谢雷, 王虹, 孙光爱. 拉伸-扭转复合加载对镍基高温合金GH4169力学性能与变形机理的影响[J]. 金属学报, 2024, 60(1): 30-42.
[8] 李时磊, 李阳, 王友康, 王胜杰, 何伦华, 孙光爱, 肖体乔, 王沿东. 基于中子与同步辐射技术的工程材料/部件多尺度残余应力评价[J]. 金属学报, 2023, 59(8): 1001-1014.
[9] 王京阳, 孙鲁超, 罗颐秀, 田志林, 任孝旻, 张洁. 以抗CMAS腐蚀为目标的稀土硅酸盐环境障涂层高熵化设计与性能提升[J]. 金属学报, 2023, 59(4): 523-536.
[10] 高钰璧, 丁雨田, 李海峰, 董洪标, 张瑞尧, 李军, 罗全顺. 变形速率对GH3625合金弹-塑性变形行为的影响[J]. 金属学报, 2022, 58(5): 695-708.
[11] 石增敏, 梁静宇, 李箭, 王毛球, 方子帆. 板条马氏体拉伸塑性行为的原位分析[J]. 金属学报, 2021, 57(5): 595-604.
[12] 李亦庄,黄明欣. 基于中子衍射和同步辐射X射线衍射的TWIP钢位错密度计算方法[J]. 金属学报, 2020, 56(4): 487-493.
[13] 毕中南,秦海龙,董志国,王相平,王鸣,刘永泉,杜金辉,张继. 高温合金盘锻件制备过程残余应力的演化规律及机制[J]. 金属学报, 2019, 55(9): 1160-1174.
[14] 秦海龙,张瑞尧,毕中南,杜洪标,张金辉. GH4169合金圆盘时效过程残余应力的演化规律研究[J]. 金属学报, 2019, 55(8): 997-1007.