Please wait a minute...
Acta Metall Sin  2020, Vol. 56 Issue (10): 1411-1422    DOI: 10.11900/0412.1961.2020.00081
Current Issue | Archive | Adv Search |
Influence of White Spot Defects on Microstructure and Mechanical Property of the GH4586 Alloy
TAN Haibing1, HUANG Shuo2(), WANG Jing1, LI Shu1, ZHU Changhong1, ZHONG Yan1, ZHONG Shilin1, HE Aijie1
1 Sichuan Gas Turbine Establishment, Aero Engine Corporation of China, Chengdu 610500, China
2 High Temperature Materials Research Division, Central Iron and Steel Research Institute, Beijing 100081, China
Cite this article: 

TAN Haibing, HUANG Shuo, WANG Jing, LI Shu, ZHU Changhong, ZHONG Yan, ZHONG Shilin, HE Aijie. Influence of White Spot Defects on Microstructure and Mechanical Property of the GH4586 Alloy. Acta Metall Sin, 2020, 56(10): 1411-1422.

Download:  HTML  PDF(4289KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

GH4586 is a nickel-based wrought superalloy developed by China, and features high Ti, W, Mo and low Al. However, it is easy to form whit spot (WP) defects within the disk components manufactured from the GH4586 ingot with a diameter of 508 mm produced by double vacuum melting method. In present work, the macro- and micro-structural characteristics, as well as the element distribution of WP defect were systematically studied. Special attention was focused on the effects of WP on mechanical properties. Hardness, tensile properties and fracture morphology of normal and defective areas were investigated for comparison. In addition, the formation mechanism and control method of WP defects were investigated based on the thermodynamic calculation and solidification simulation, respectively. In order to analyze its dendritic segregation and second phase precipitation in the solidification process, solidification phase diagram and thermodynamic equilibrium phase diagram of GH4586 alloy were calculated with JmatPro software. To study the forming mechanism of WP, the solidification process of vacuum introduction melting (VIM) GH4586 ingots was simulated with Procast software. Results show that the WP defects within GH4586 components are dendritic WP which exhibits dendritic pattern on the macro level. While on micro level, it is the precipitate clusters which consisted of MC carbides, M6C carbides and large incoherent γ′ phase. Due to the clusters' inherent rigid and fragile characteristics, the tensile strength and ductility of the alloy are significantly reduced. Therefore, the WP defects are harmful to the mechanical properties of the GH4586 disk significantly. The WP defects must be avoided during the forging process. Since excessive internal stress and shrinkage cavities form during the solidification process of large VIM GH4586 ingots, chips fall into molten pool easily if the VIM ingots are employed as vacuum arc remelting (VAR) electrode, and then give birth to WP defects within the final forging components. Therefore, it is the effective method for avoiding WP defects by improving the quality of VAR electrode and optimizing the VAR process.

Key words:  nickel-based wrought superalloy      GH4586 alloy      white spot defect      structure      mechanical property     
Received:  13 March 2020     
ZTFLH:  TG146.1  
Fund: National Science and Technology Major Project(2017-VI-0015-0087);National Science and Technology Major Project(2017-VI-0018-0090)

URL: 

https://www.ams.org.cn/EN/10.11900/0412.1961.2020.00081     OR     https://www.ams.org.cn/EN/Y2020/V56/I10/1411

AlloyCCrCoTiAlWMoNbFeNi
GH45860.0619.011.03.201.63.08.0--Bal.
GH41410.0615.011.03.101.5-9.5--Bal.
GH41690.0319.0-0.950.5-3.05.2Bal.52.5
GH47380.0319.513.53.101.4-4.3--Bal.
Table 1  Nominal compositions of typical wrought superalloy for disk forging
Fig.1  Typical macro morphologies of white spot defects in the GH4586 alloy disk
(a) polished (b) etched
Fig.2  OM (a), SEM-BSE (b, c) and SEM-SE (d~f) images showing typical micro morphologies of white spot defects in the GH4586 alloy disk
Fig.3  EPMA elemental maps of the white spot defect corresponding to Fig.2a
Color online
Fig.4  EPMA elemental maps of white spot defect corresponding to Fig.2c
Color online
Fig.5  TEM image (a) and SAED patterns of positions P1 (b), P2 (c) and P3 (d) of the precipitate clusters in white spot defect shown in the Fig.2d with the wire frame
PositionCAlTiCrCoNiMoW
P10.30±0.179.29±2.4214.39±3.102.24±0.485.59±1.2167.62±14.600.44±0.110.14±0.03
P27.72±0.951.31±0.305.25±0.9023.20±3.9610.25±1.7522.61±3.8623.29±4.276.37±0.97
P347.49±5.940.26±0.0642.24±7.700.53±0.100.15±0.030.44±0.087.01±1.361.88±0.31
Table 2  EDS analysis results of positions P1, P2 and P3 shown in Fig.5a

Area

Hardness / HVσb / MPaσ0.2 / MPaδ / %ψ / %
Aver.Stand. deviationAver.Stand. deviationAver.Stand. deviationAver.Stand. deviationAver.Stand. deviation
Normal44615.52148738.21110718.8118.53.8816.03.00
Defect52916.3111797.4110881.730.50.282.00.57
Table 3  Vickers hardnesses and room temperature tensile properties of the white spot defect area and normal area
Fig.6  Typical fracture morphology (a) and the morphology of longitudinal section nearby the fracture (b) of the tensile sample with white spot defect
Fig.7  Solidification phase diagram (a), thermodynamic phase diagram (b) and element fraction of liquid during the solidification (c) of the GH4586 alloy calculated by Jmatpro
PhaseMethodNiAlCoCrMoTiWC
MCSPD---0.200.3752.250.6246.56
σSPD23.470.0511.4639.1325.49-0.39-
ηSPD66.371.918.760.27-22.70--
MCTPD---0.350.3348.702.6747.95
σTPD16.520.0018.9554.899.51-0.13-
γ′TPD71.9510.233.151.800.0912.390.40-
M6CTPD26.60-2.8420.1932.89-3.1914.29
M23C6TPD3.02-1.2864.9610.000.000.04-
PTPD27.34-7.7430.7625.01-9.15-
μTPD23.82-21.1420.5329.54-4.97
Table 4  Compositions of second phases in the solidification phase diagram and thermodynamic phase diagram of the GH4586 alloy calculated by Jmatpro software
Fig.8  EPMA elemental maps of vacuum induction melting (VIM) ingot sample of GH4586 alloy
Color online
Fig.9  Numerical simulations of the solidification process of GH4586 alloy VIM ingot for pouring by 1/4 (a1~d1), pouring end (a2~d2), cool for t1 (a3~d3), cool for t2 (a4~d4) and cool for t3 (a5~d5), which t1, t2 and t3 mean the cooling time increased
Color online
(a1~a5) temperature (b1~b5) mass fraction of solid phase (c1~c5) effective stress (d1~d5) total shrinkage porosity
Fig.10  SEM-SE (a) and SEM-BSE (b) images showing typical morphologies of the shrinkage porosity in GH4586 alloy VIM ingot
[1] Zhang B J, Zhao G P, Jiao L Y, et al. Influence of hot working process on microstructures of superalloy GH4586 [J]. Acta Metall. Sin., 2005, 41: 351
(张北江, 赵光普, 焦兰英等. 热加工工艺对GH4586合金微观组织的影响 [J]. 金属学报, 2005, 41: 351)
[2] Wang L, Wang S, Song X, et al. Effects of precipitated phases on the crack propagation behaviour of a Ni-based superalloy [J]. Int. J. Fatigue, 2014, 62: 210
doi: 10.1016/j.ijfatigue.2013.10.006
[3] Wang S, Wang L, Liu Y, et al. Effect of long-term aging on the fatigue crack growth rate of a nickel-based superalloy [J]. Mater. Sci. Eng., 2011, A528: 2110
[4] Fecht H, Furrer D. Processing of nickel-base superalloys for turbine engine disc applications [J]. Adv. Eng. Mater., 2000, 2: 777
doi: 10.1002/(ISSN)1527-2648
[5] Du J H, Lv X D, Dong J X, et al. Research progress of wrought superalloys in China [J]. Acta Metall. Sin., 2019, 55: 1115
doi: 10.11900/0412.1961.2019.00142
(杜金辉, 吕旭东, 董建新等. 国内变形高温合金研制进展 [J]. 金属学报, 2019, 55: 1115)
doi: 10.11900/0412.1961.2019.00142
[6] Xu G H, Jiao L Y, Zhang B J, et al. Effect of cooling rate after solid solution on microstructure and tensile properties of GH4586 superalloy at 850 ℃ [J]. Trans. Mater. Heat Treat., 2006, 27: 47
(胥国华, 焦兰英, 张北江等. 固溶冷却速度对GH4586合金组织及850 ℃拉伸性能的影响 [J]. 材料热处理学报, 2006, 27: 47)
[7] Zhong Z Y, Zhuang J Y. Development of several important problems on producing technologies of wrought superalloy [J]. J. Iron Steel Res., 2003, 15(7): 1
(仲增墉, 庄景云. 变形高温合金生产工艺中几个重要问题的研究和进展 [J]. 钢铁研究学报, 2003, 15(7): 1)
[8] Liu Q M, Huang S Z, Chen Y L, et al. Investigation on the abnormal corrosion spots of GH4169G alloy parts [J]. Gas Turb. Exp. Res., 2019, 32: 52
(刘巧沐, 黄顺洲, 陈玉龙等. GH4169G合金零件异常腐蚀区缺陷分析 [J]. 燃气涡轮试验与研究, 2019, 32: 52)
[9] Reed R C. The Superalloys Fundamentals and Applications [M]. New York: Cambridge University Press, 2006: 222
[10] Jackman L A, Maurer G E, Widge S. White spots in superalloys [A]. Superalloys 718, 625, 706 and Various Derivatives [C]. Warrendale, PA: TMS, 1994: 153
[11] Zhang B J, Huang S, Zhang W Y, et al. Recent development of nickel-based disc alloys and corresponding cast-wrought processing techniques [J]. Acta Metall. Sin., 2019, 55: 1095
doi: 10.11900/0412.1961.2019.00078
(张北江, 黄 烁, 张文云等. 变形高温合金盘材及其制备技术研究进展 [J]. 金属学报, 2019, 55: 1095)
doi: 10.11900/0412.1961.2019.00078
[12] Huang Q Y, Li H K. Superalloy [M]. Beijing: Metallurgical Industry Press, 2000: 186
(黄乾尧, 李汉康. 高温合金 [M]. 北京: 冶金工业出版社, 2000: 186)
[13] Scarfo J P, Wolski K, Gros V, et al. Powerplant group chairman's factual report [R]. Washington: National Transportation Safety Board, 2017
[14] Damkroger B K, Kelley J B, Schlienger M E, et al. The influence of VAR processes and parameters on white spot formation in alloy 718 [A]. Superalloys 718, 625, 706 and Various Derivatives [C]. Warrendale, PA: TMS, 1994: 125
[15] Grignard J F, Soller A, Jourdan J, et al. On the formation of white-spot defects in a superalloy VAR ingot [J]. Adv. Eng. Mater., 2011, 13: 563
doi: 10.1002/adem.v13.7
[16] Li L H, Dong J X, Zhang M C, et al. Integrated simulation of the forging process for GH4738 alloy turbine disk and its application [J]. Acta Metall. Sin., 2014, 50: 821
doi: 10.3724/SP.J.1037.2013.00675
(李林翰, 董建新, 张麦仓等. GH4738合金涡轮盘锻造过程的集成式模拟及应用 [J]. 金属学报, 2014, 50: 821)
doi: 10.3724/SP.J.1037.2013.00675
[17] Samuelsson E, Domingue J A, Maurer G E. Characterizing solute-lean defects in superalloys [J]. JOM, 1990, 42(8): 27
[18] Wang Z X, Huang S, Zhang B J, et al. Study on freckle of a high-alloyed GH4065 nickel base wrought superalloy [J]. Acta Metall. Sin., 2019, 55: 417
doi: 10.11900/0412.1961.2018.00218
(王资兴, 黄 烁, 张北江等. 高合金化GH4065镍基变形高温合金点状偏析研究 [J]. 金属学报, 2019, 55: 417)
doi: 10.11900/0412.1961.2018.00218
[19] Dong J X, Li A, Zhang M C. Thermodynamic simulation of precipitations in GH586 superalloy [J]. J. Mater. Eng., 2003, (9): 7
(董建新, 李 昂, 张麦仓. GH586高温合金析出相的热力学模拟计算 [J]. 材料工程, 2003, (9): 7)
[20] Zhuang J Y, Du J H, Deng Q, et al. Wrought Superalloy GH4169 [M]. Beijing: Metallurgical Industry Press, 2006: 19
(庄景云, 杜金辉, 邓 群等. 变形高温合金GH4169 [M]. 北京: 冶金工业出版社, 2006: 19)
[21] Jones R M F, Jackman L A. The structural evolution of superalloy ingots during hot working [J]. JOM, 1999, 51(1): 27
[22] Moyer J M, Jackman L A, Adasczik C B, et al. Advances in triple melting superalloys 718, 706, and 720 [A]. Superalloys 718, 625, 706 and Various Derivatives [C]. Warrendale, PA: TMS, 1994: 39
[23] Dong J X, Li L H, Li R Y, et al. Effect of extent of homogenization on the hot deformation recrystallization of superalloy ingot in cogging process [J]. Acta Metall. Sin., 2015, 51: 1207
doi: 10.11900/0412.1961.2015.00419
(董建新, 李林翰, 李浩宇等. 高温合金铸锭均匀化程度对开坯热变形的再结晶影响 [J]. 金属学报, 2015, 51: 1207)
doi: 10.11900/0412.1961.2015.00419
[24] Xie S S, Yang H C, Wang Z X, et al. Effects of grain-boundary carbides on high-temperature strength in the superalloy GH586 [J]. J. Northeast. Univ. (Nat. Sci.), 1998, 19: 577
(谢世殊, 杨洪才, 王志兴等. GH586合金的晶界碳化物高温强化 [J]. 东北大学学报(自然科学版), 1998, 19: 577)
[25] Van Den Avyle J A, Brooks J A, Powell A C. Reducing defects in remelting processes for high-performance alloys [J]. JOM, 1998, 50(3): 22
[26] Zhang B J, Zhao G P, Zhang W Y, et al. Investigation of high performance disc alloy GH4065 and associated advanced processing techniques [J]. Acta Metall. Sin., 2015, 51: 1227
doi: 10.11900/0412.1961.2015.00368
(张北江, 赵光普, 张文云等. 高性能涡轮盘材料GH4065及其先进制备技术研究 [J]. 金属学报, 2015, 51: 1227)
doi: 10.11900/0412.1961.2015.00368
[27] Crozet C, Devaux A, Forestier R, et al. Effect of ingot size on microstructure and properties of the new advanced AD730TM superalloy [A]. Superalloys 2016: Proceedings of the 13th Intenational Symposium of Superalloys [C]. Warrendale, PA: TMS, 2016: 437
[1] WANG Lei, LIU Mengya, LIU Yang, SONG Xiu, MENG Fanqiang. Research Progress on Surface Impact Strengthening Mechanisms and Application of Nickel-Based Superalloys[J]. 金属学报, 2023, 59(9): 1173-1189.
[2] MA Dexin, ZHAO Yunxing, XU Weitai, WANG Fu. Effect of Gravity on Directionally Solidified Structure of Superalloys[J]. 金属学报, 2023, 59(9): 1279-1290.
[3] ZHANG Jian, WANG Li, XIE Guang, WANG Dong, SHEN Jian, LU Yuzhang, HUANG Yaqi, LI Yawei. Recent Progress in Research and Development of Nickel-Based Single Crystal Superalloys[J]. 金属学报, 2023, 59(9): 1109-1124.
[4] ZHENG Liang, ZHANG Qiang, LI Zhou, ZHANG Guoqing. Effects of Oxygen Increasing/Decreasing Processes on Surface Characteristics of Superalloy Powders and Properties of Their Bulk Alloy Counterparts: Powders Storage and Degassing[J]. 金属学报, 2023, 59(9): 1265-1278.
[5] GONG Shengkai, LIU Yuan, GENG Lilun, RU Yi, ZHAO Wenyue, PEI Yanling, LI Shusuo. Advances in the Regulation and Interfacial Behavior of Coatings/Superalloys[J]. 金属学报, 2023, 59(9): 1097-1108.
[6] ZHANG Leilei, CHEN Jingyang, TANG Xin, XIAO Chengbo, ZHANG Mingjun, YANG Qing. Evolution of Microstructures and Mechanical Properties of K439B Superalloy During Long-Term Aging at 800oC[J]. 金属学报, 2023, 59(9): 1253-1264.
[7] LU Nannan, GUO Yimo, YANG Shulin, LIANG Jingjing, ZHOU Yizhou, SUN Xiaofeng, LI Jinguo. Formation Mechanisms of Hot Cracks in Laser Additive Repairing Single Crystal Superalloys[J]. 金属学报, 2023, 59(9): 1243-1252.
[8] DING Hua, ZHANG Yu, CAI Minghui, TANG Zhengyou. Research Progress and Prospects of Austenite-Based Fe-Mn-Al-C Lightweight Steels[J]. 金属学报, 2023, 59(8): 1027-1041.
[9] LI Jingren, XIE Dongsheng, ZHANG Dongdong, XIE Hongbo, PAN Hucheng, REN Yuping, QIN Gaowu. Microstructure Evolution Mechanism of New Low-Alloyed High-Strength Mg-0.2Ce-0.2Ca Alloy During Extrusion[J]. 金属学报, 2023, 59(8): 1087-1096.
[10] CHEN Liqing, LI Xing, ZHAO Yang, WANG Shuai, FENG Yang. Overview of Research and Development of High-Manganese Damping Steel with Integrated Structure and Function[J]. 金属学报, 2023, 59(8): 1015-1026.
[11] LIU Xingjun, WEI Zhenbang, LU Yong, HAN Jiajia, SHI Rongpei, WANG Cuiping. Progress on the Diffusion Kinetics of Novel Co-based and Nb-Si-based Superalloys[J]. 金属学报, 2023, 59(8): 969-985.
[12] YUAN Jianghuai, WANG Zhenyu, MA Guanshui, ZHOU Guangxue, CHENG Xiaoying, WANG Aiying. Effect of Phase-Structure Evolution on Mechanical Properties of Cr2AlC Coating[J]. 金属学报, 2023, 59(7): 961-968.
[13] SUN Rongrong, YAO Meiyi, WANG Haoyu, ZHANG Wenhuai, HU Lijuan, QIU Yunlong, LIN Xiaodong, XIE Yaoping, YANG Jian, DONG Jianxin, CHENG Guoguang. High-Temperature Steam Oxidation Behavior of Fe22Cr5Al3Mo-xY Alloy Under Simulated LOCA Condition[J]. 金属学报, 2023, 59(7): 915-925.
[14] ZHANG Deyin, HAO Xu, JIA Baorui, WU Haoyang, QIN Mingli, QU Xuanhui. Effects of Y2O3 Content on Properties of Fe-Y2O3 Nanocomposite Powders Synthesized by a Combustion-Based Route[J]. 金属学报, 2023, 59(6): 757-766.
[15] GUO Fu, DU Yihui, JI Xiaoliang, WANG Yishu. Recent Progress on Thermo-Mechanical Reliability of Sn-Based Alloys and Composite Solder for Microelectronic Interconnection[J]. 金属学报, 2023, 59(6): 744-756.
No Suggested Reading articles found!