Please wait a minute...
Acta Metall Sin  2018, Vol. 54 Issue (10): 1387-1398    DOI: 10.11900/0412.1961.2018.00100
Current Issue | Archive | Adv Search |
Microstructure and Mechanical Properties of an Austenite/Ferrite Laminate Structured High-Manganese Steel
Kai ZHU, Cuilan WU(), Pan XIE, Mei HAN, Yuanrui LIU, Xiangge ZHANG, Jianghua CHEN
College of Materials Science and Engineering, Hunan University, Changsha 410082, China
Cite this article: 

Kai ZHU, Cuilan WU, Pan XIE, Mei HAN, Yuanrui LIU, Xiangge ZHANG, Jianghua CHEN. Microstructure and Mechanical Properties of an Austenite/Ferrite Laminate Structured High-Manganese Steel. Acta Metall Sin, 2018, 54(10): 1387-1398.

Download:  HTML  PDF(13511KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

Lamianate structured metals have recently attracted extensive interests for their outstanding mechanical properties which are produced by synergetic strengthening of different heterogeneous layers. For Mn-rich maraging steels, austenite can precipitate in the martensite matrix due to Mn segregation during heat treatment, and then the austenite and martensite/ferrite duplex steel is produced. Besides, high Mn TRIP steel is regarded as a promising material for next generation automobile steel because of its high strength and good ductility. In this work, the microstructures and properties of Mn12Ni2MoTi(Al) steels produced by thermo-mechanical process were investigated using XRD, SEM, TEM, EBSD, EPMA, hardness tests and tensile tests. The results showed that laminate structures with austenite/ferrite band alternate arranging along the normal direction were formed in Mn12Ni2MoTi(Al) steels, which were processed by 65% cold-rolling and subsequent annealing at 745 ℃. Both of austenite bands and ferrite bands consist of ultrafine equiaxed grains. Moreover, a small amount of ferrite grains and austenite grains were found inside the austenite bands and ferrite bands, respectively. In the austenite/ferrite laminate structures, the austenite bands show the Brass texture of {110}<112> and Goss- type texture of {110}<001>. The ferrite bands show the rotate Cube texture of {001} <110> and Cube texture of {001}<100>. With the increase of annealing time, the laminate structures first become dominant and then disappear gradually, accompanying with the orientation transition of austenite from the Brass texture into the Goss one. The samples with laminate structures have high yield strength and good ductility. Otherwise, when the laminate structures disappear, the yield strength and ductility of the samples will decrease, and the yield strength deceases more.

Key words:  laminate structure      high manganese steel      thermomechanical process      TRIP effect     
Received:  19 March 2018     
ZTFLH:  TG166.7  
Fund: Supported by National Natural Science Foundation of China (Nos.11427806 and 51371081)

URL: 

https://www.ams.org.cn/EN/10.11900/0412.1961.2018.00100     OR     https://www.ams.org.cn/EN/Y2018/V54/I10/1387

Fig.1  Schematic of a sample (ND-section, TD-section and RD-section are perpendicular to the normal direction, the transverse direction and the rolling direction, respectively)
Texture component Symbol Miller index
Cube ■ {001}<100>
Rotated Cube ◇ {001}<110>
Goss ▲ {110}<001>
Brass ● {110}<112>
E-typed ★ {111}<110>
F-typed ☆ {111}<112>
Copper {112}<111>
Rotated Goss {110}<110>
Table 1  The Miller indices and texture components of symbols given in Fig.2
Fig.2  Locations of common textures components of metals in the ψ2=0° and ψ2=45° sections (The Miller indices and texture components of symbols are given in Table 1)[29]
Fig.3  TEM image (a), ND-sectional XRD spectrum (b) and ODFs of texture at ψ2=0° (c) and ψ2=45° (d) of 65%CR sample
Fig.4  SEM images of 745 ℃-1 h sample in different sections
(a) ND-section (b) TD-section (c) RD-section (d) low magnified image of the TD-section
Fig.5  The average thickness curves (a) and Vickers hardness curves (b) of bright bands and dark bands in the same samples annealed for different time at 745 ℃ (Inset shows the indentations of different bands)
Fig.6  SEM image (a) and EBSD phase-map (b) of the 745 ℃-1 h sample
Fig.7  XRD spectra of 745 ℃-1 h annealed samples in different sections
Fig.8  The relative volume fraction of γ in the samples annealed at 745 ℃ for different time
Fig.9  EBSD phase-maps (a~f) and IPF-maps (a1~f1) of the samples annealed at 745 ℃ for different time (In the EBSD phase-maps, the red represents the austenite while the green represents the ferrite. In the IPF-maps, different colours represent different directions of grains)
(a, a1) 745 ℃-5 min (b, b1) 745 ℃-30 min (c, c1, e, e1, f, f1) 745 ℃-1 h (d, d1) 745 ℃-24 h
Fig.10  Textures of austenite in the different samples annealed for different time at 745 ℃
(a, a1) 745 ℃-5 min (b, b1) 745 ℃-30 min (c, c1) 745 ℃-1 h (d, d1) 745 ℃-24 h
Fig.11  Textures of ferrite in the different samples annealed for different time at 745 ℃
(a, a1) 745 ℃-5 min (b, b1) 745 ℃-30 min (c, c1) 745 ℃-1 h (d, d1) 745 ℃-24 h
Fig.12  EPMA maps of Mn distribution for different samples
(a) 65%CR (b) 745 ℃-30 min (c) 745 ℃-24 h
Fig.13  TEM images of 745 ℃-1 h (a, c) and 745 ℃-24 h (b, d) samples (a, b) recrystallized grains (c, d) martensite
Fig.14  Tensile stress-strain curves of different samples
Fig.15  EBSD phase-maps (a~d) and IPF-maps (a1~d1) of the 745 ℃-1 h sample with different tensile deformations (In the EBSD phase-maps, the red represents the austenite while the green represents the ferrite. In the IPF-maps, different colours represent different directions of grains)
(a, a1) 0.5% strain (b, b1) 5% strain (c, c1) 10% strain (d, d1) tensile fracture
Fig.16  EBSD phase-map (a) and IPF-map (a1) of the 745 ℃-24 h sample after tensile fracture (In the EBSD phase-maps, the red represents the austenite while the green represents the ferrite. In the IPF-maps, different colours represent different directions of grains)
[1] Latypov M I, Shin S, De Cooman B C, et al. Micromechanical finite element analysis of strain partitioning in multiphase medium manganese TWIP+TRIP steel[J]. Acta Mater., 2016, 108: 219
[2] Frommeyer G, Brüx U, Neumann P, et al.Supra-ductile and high-strength manganese-TRIP/TWIP steels for high energy absorption purposes[J]. ISIJ Int., 2003, 43: 438
[3] Li K, Injeti V S Y, Misra R D K, et al. On the strain rate sensitivity of aluminum-containing transformation-induced plasticity steels: Interplay between TRIP and TWIP effects[J]. Mater. Sci. Eng., 2017, A711: 515
[4] Allain S, Chateau J P, Dahmoun D, et al. Modeling of mechanical twinning in a high manganese content austenitic steel [J]. Mater. Sci. Eng., 2004, A387-389: 272
[5] Bouaziz O, Guelton N. Modelling of TWIP effect on work-hardening [J]. Mater. Sci. Eng., 2001, A319-321: 246
[6] Wang Y M, Chen M W, Sheng H W, et al.Nanocrystalline grain structures developed in commercial purity Cu by low-temperature cold rolling[J]. J. Mater. Res., 2002, 17: 3004
[7] Huang X X, Hansen N, Tsuji N.Hardening by annealing and softening by deformation in nanostructured metals[J]. Science, 2006, 312: 249
[8] Valiev R.Nanostructuring of metals by severe plastic deformation for advanced properties[J]. Nat. Mater., 2004, 3: 511
[9] Wu X L, Yang M X, Yuan F P, et al.Heterogeneous lamella structure unites ultrafine-grain strength with coarse-grain ductility[J]. Proc. Natl. Acad. Sci. U. S. A., 2015, 112: 14501
[10] Wang Y M, Ma E.Three strategies to achieve uniform tensile deformation in a nanostructured metal[J]. Acta Mater., 2004, 52: 1699
[11] Song R, Ponge D, Raabe D, et al.Overview of processing, microstructure and mechanical properties of ultrafine grained bcc steels[J]. Mater. Sci. Eng., 2006, A441: 1
[12] Rezaee A, Kermanpur A, Najafizadeh A, et al.Production of nano/ultrafine grained AISI 201L stainless steel through advanced thermo-mechanical treatment[J]. Mater. Sci. Eng., 2011, A528: 5025
[13] Forouzan F, Najafizadeh A, Kermanpur A, et al.Production of nano/submicron grained AISI 304L stainless steel through the martensite reversion process[J]. Mater. Sci. Eng., 2010, A527: 7334
[14] Dini G, Najafizadeh A, Monir-Vaghefi S M, et al. Grain size effect on the martensite formation in a high-manganese TWIP steel by the Rietveld method[J]. J. Mater. Sci. Technol., 2010, 26: 181
[15] Yin Y Q, Wu C L, Xie P, et al.An ultrafine grained duplex Mn12Ni2MoTi(Al) steel fabricated by cold rolling and annealing[J]. Acta Metall. Sin., 2016, 52: 1527(尹炎祺, 伍翠兰, 谢盼等. 冷轧及退火制备的超细晶粒双相Mn12Ni2MoTi(Al)钢[J]. 金属学报, 2016, 52: 1527)
[16] Tsuji N, Ueji R, Minamino Y, et al.A new and simple process to obtain nano-structured bulk low-carbon steel with superior mechanical property[J]. Scr. Mater., 2002, 46: 305
[17] Eizadjou M, Talachi A K, Manesh H D, et al.Investigation of structure and mechanical properties of multi-layered Al/Cu composite produced by accumulative roll bonding (ARB) process[J]. Compos. Sci. Technol., 2008, 68: 2003
[18] Fang T H, Li W L, Tao N R, et al.Revealing extraordinary intrinsic tensile plasticity in gradient nano-grained copper[J]. Science, 2011, 331: 1587
[19] Tan H F, Zhang B, Luo X M, et al.Strain rate dependent tensile plasticity of ultrafine-grained Cu/Ni laminated composites[J]. Mater. Sci. Eng., 2014, A609: 318
[20] Lee H, Min C J, Sohn S S, et al.Novel medium-Mn (austenite+martensite) duplex hot-rolled steel achieving 1.6GPa strength with 20% ductility by Mn-segregation-induced TRIP mechanism[J]. Acta Mater., 2018, 147: 247
[21] Ueji R, Tsuji N, Minamino Y, et al.Effect of rolling reduction on ultrafine grained structure and mechanical properties of low-carbon steel thermomechanically processed from martensite starting structure[J]. Sci. Technol. Adv. Mater., 2004, 5: 153
[22] Wu X L, Yang M X, Yuan F P, et al.Combining gradient structure and TRIP effect to produce austenite stainless steel with high strength and ductility[J]. Acta Mater., 2016, 112: 337
[23] Ma X L, Huang C X, Moering J, et al.Mechanical properties of copper/bronze laminates: Role of interfaces[J]. Acta Mater., 2016, 116: 43
[24] Zhang L, Chen Z, Wang Y H, et al.Fabricating interstitial-free steel with simultaneous high strength and good ductility with homogeneous layer and almella structure[J]. Scr. Mater., 2017, 141: 111
[25] Chen H, Zhang C Y, Zhu J N, et al.Austenite/ferrite interface migration and alloying elements partitioning: An overview[J]. Acta Metall. Sin., 2018, 54: 217(陈浩, 张璁雨, 朱加宁等. 奥氏体/铁素体界面迁移与元素配分的研究进展[J]. 金属学报, 2018, 54: 217)
[26] Xie P, Han M, Wu C L, et al.A high-performance TRIP steel enhanced by ultrafine grains and hardening precipitates[J]. Mater. Des., 2017, 127: 1
[27] De Amar K, Murdock D C, Mataya M C, et al.Quantitative measurement of deformation-induced martensite in 304 stainless steel by X-ray diffraction[J]. Scr. Mater., 2004, 50: 1445
[28] Chen Y, Wu C L, Xie P, et al.A phase-transformation-strengthened surface layer on Fe-20Mn-3Al-3Si steel fabricated by mechanical grinding[J]. Acta Metall. Sin., 2014, 50: 423(陈燕, 伍翠兰, 谢盼等. 机械磨擦制备的Fe-20Mn-3Al-3Si钢表面相变强化层[J]. 金属学报, 2014, 50: 423)
[29] Xu H J, Xu Y B, Jiao H T, et al.Influence of grain size and texture prior to warm rolling on microstructure, texture and magnetic properties of Fe-6.5%wt%Si steel[J]. J. Magn. Magn. Mater., 2018, 453: 236
[30] De Moor E, Matlock D K, Speer J G, et al.Austenite stabilization through manganese enrichment[J]. Scr. Mater., 2011, 64: 185
[31] Lee S, Kim J, Lee S J, et al.Effect of nitrogen on the critical strain for dynamic strain aging in high-manganese twinning-induced plasticity steel[J]. Scr. Mater., 2011, 65: 528
[32] Oh K H, Jeong J S, Koo Y M, et al.The evolution of the rolling and recrystallization textures in cold-rolled Al containing high Mn austenitic steels[J]. Mater. Chem. Phys., 2015, 161: 9
[33] Lee D A.Elastic properties of thin films of cubic system[J]. Thin Solid Films, 2003, 434: 183
[34] Lee D A.A stability criterion for deformation and deposition textures of metals during annealing[J]. J. Mater. Process. Technol., 2001, 117: 307
[1] WANG Bin, NIU Mengchao, WANG Wei, JIANG Tao, LUAN Junhua, YANG Ke. Microstructure and Strength-Toughness of a Cu-Contained Maraging Stainless Steel[J]. 金属学报, 2023, 59(5): 636-646.
[2] WANG Shihong,LI Jian,GE Xin,CHAI Feng,LUO Xiaobing,YANG Caifu,SU Hang. Microstructural Evolution and Work Hardening Behavior of Fe-19Mn Alloy Containing Duplex Austenite and ε-Martensite[J]. 金属学报, 2020, 56(3): 311-320.
[3] Miao JIN, Wenquan LI, Shuo HAO, Ruixue MEI, Na LI, Lei CHEN. Effect of Solution Temperature on Tensile Deformation Behavior of Mn-N Bearing Duplex Stainless Steel[J]. 金属学报, 2019, 55(4): 436-444.
[4] Yaqiang TIAN,Geng TIAN,Xiaoping ZHENG,Liansheng CHEN,Yong XU,Shihong ZHANG. C and Mn Elements Characterization and Stability of Retained Austenite in Different Locations ofQuenching and Partitioning Bainite Steels[J]. 金属学报, 2019, 55(3): 332-340.
[5] CHEN Lei, HAO Shuo, ZOU Zongyuan, HAN Shuting, ZHANG Rongqiang, GUO Baofeng. Mechanical Characteristics of TRIP-Assisted Duplex Stainless Steel Fe-19.6Cr-2Ni-2.9Mn-1.6Si During Cyclic Deformation[J]. 金属学报, 2019, 55(12): 1495-1502.
[6] CHEN Lei , HAO Shuo , MEI Ruixue , JIA Wei , LI Wenquan , GUO Baofeng . Intrinsic Increment of Plasticity Induced by TRIP and Its Dependence on the Annealing Temperature in a Lean Duplex Stainless Steel[J]. 金属学报, 2019, 55(11): 1359-1366.
[7] Feng YANG, Haiwen LUO, Han DONG. Effects of Intercritical Annealing Temperature on the Tensile Behavior of Cold Rolled 7Mn Steel and the Constitutive Modeling[J]. 金属学报, 2018, 54(6): 859-867.
[8] Dongdong LI, Lihe QIAN, Shuai LIU, Jiangying MENG, Fucheng ZHANG. Effect of Manganese Content on Tensile Deformation Behavior of Fe-Mn-C TWIP Steels[J]. 金属学报, 2018, 54(12): 1777-1784.
[9] Yi CHEN, Mingxing GUO, Long YI, Bo YUAN, Gaojie LI, Linzhong ZHUANG, Jishan ZHANG. Optimization and Controlling on the Microstructure, Texture and Properties of an Advanced Al-Mg-Si-Cu-Zn Alloy Sheet[J]. 金属学报, 2017, 53(8): 907-917.
[10] Lina WANG,Ping YANG,Weimin MAO. ANALYSIS OF MARTENSITIC TRANSFORMATIONDURING TENSION OF HIGH MANGANESETRIP STEEL AT HIGH STRAIN RATES[J]. 金属学报, 2016, 52(9): 1045-1052.
[11] Yan ZHANG,Mingxing GUO,Hui XING,Fei WANG,Xiaofeng WANG,Jishan ZHANG,Linzhong ZHUANG. INFLUENCE OF DIFFERENT THERMOMECHANICAL PROCESSES ON THE MECHANICAL PROPERTIES AND MICROSTRUCTURE OF Al-Mg-Si-Cu ALLOY SHEETS[J]. 金属学报, 2015, 51(12): 1425-1434.
[12] CHEN Yan, WU Cuilan, XIE Pan, CHEN Wanglin, XIAO Hui, CHEN Jianghua. A PHASE-TRANSFORMATION-STRENGTHENED SURFACE LAYER ON Fe-20Mn-3Al-3Si STEEL FABRICATED BY MECHANICAL GRINDING[J]. 金属学报, 2014, 50(4): 423-430.
[13] REN Yongqiang XIE Zhenjia SHANG Chengjia. REGULATION OF RETAINED AUSTENITE AND ITS EFFECT ON THE MECHANICAL PROPERTIES OF LOW CARBON STEEL[J]. 金属学报, 2012, 48(9): 1074-1080.
[14] WEN Yuhua ZHANG Wanhu SI Haitao XIONG Renlong PENG Huabei. STUDY ON WORK HARDENING BEHAVIOUR AND MECHANISM OF HIGH SILICON AUSTENITIC HIGH MANGANESE STEEL[J]. 金属学报, 2012, 48(10): 1153-1159.
[15] YANG Ping LU Fayun MENG Li CUI Feng’e. εCRYSTALLOGRAPHIC BEHAVIORS OF COMPRESSED HIGH MANGANESE TRIP/TWIP STEELS ANALYZED BY EBSD TECHNIQUES
I. Transformation Characteristics, Twinning and the Influence of Austenitic Orientations