LIU Wenhui; LIU Yangai; XONG Shoumei; LIU Baicheng; Y. Matsumoto; M. Murakami. Comparative Study of the Cavity Pressure of Magnesium Alloy and Aluminium Alloy During Die Casting Process. Acta Metall Sin, 2005, 41(1): 103-.
Abstract The pressure changes in the cavity of ADC12 and
AZ91D die castings under the same processing technology
have been measured. From liquid phase to solid phase, the pressure
curves of ADC12 and AZ91D are divided into six sections and the
characteristic parameters were defined based on the experimental
results. The results show that the filling pressure and filling
time as well as the trend of pressure change of these two alloys
are almost the same. The pressure holding time and the effective
holding time of the transferred pressure of ADC12 are much higher
than those of AZ91D. For different measured points, the
maximum transferred pressures of ADC12 are close to each other
and those of AZ91D show a great difference. The difference of
pressure curves between the two alloys is related to the
solidification characteristic of the liquid
metal and the mechanical properties of the alloys.
[1] Tanikawa D, Asai K, Nomura H, Kato E. 2002 Japan Die Casting Congress, 2002: 145 [2] Kubota S, Fujimaki D, Katoh T. 2002 Japan Die Casting Congress, 2002: 187 [3] Tong K S, Hu B H, Niu X P. J Mater Proc Technol, 2002; 127: 238 [4] Lin B N. Foundry Rheology. Harbin: Press of Harbin In- stitute of Technology, 1991: 108 (林柏年.铸造流变学.哈尔滨:哈尔滨工业大学出版社.1991: 108) . [5] Li D F, Wang Z D. Nonferrous Met, 1997; (5): 4 (李德富,王志东.有色金属, 1997;(5):4) [6] Cheng J, Dang J Z, Cheng M, Zhao J P. J North Chin Inst Technol, 1995; (1): 9 (程军,党惊知,程眉,赵建平.华北工学院学报,1995; (1):9) [7] Wang B D, Liu Y, Li D F, Wang B X, Wang Z T. Met Forming Technol, 2003; (2): 40 (王炳德,刘莹,李德富,王本贤,王忠堂.金属成型工艺, 2003;(2):40)c