Please wait a minute...
Acta Metall Sin  1998, Vol. 34 Issue (6): 621-626    DOI:
Current Issue | Archive | Adv Search |
CHAJRACTERISTICS OF OXIDE FORMED ON THE SURFACE OF Zn-48.48Al-1.65Cu-0.03Mg MELT
CHEN Yunwi; TU Mingjing(Department of Metal Materials; Sichuan Union University; Chengdu 610065)Correspondent: CHEN Yungui; associate professor Tel.(028)5405701; Fax:(028)5220670
Cite this article: 

CHEN Yunwi; TU Mingjing(Department of Metal Materials; Sichuan Union University; Chengdu 610065)Correspondent: CHEN Yungui; associate professor Tel.(028)5405701; Fax:(028)5220670. CHAJRACTERISTICS OF OXIDE FORMED ON THE SURFACE OF Zn-48.48Al-1.65Cu-0.03Mg MELT. Acta Metall Sin, 1998, 34(6): 621-626.

Download:  PDF(546KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  The hoe characteristics of the Oxide am on the surface of Zn -- 48. 48Al -- 1. 6 5 Cu 0.03Mg meltl were investigated using X--ray photoelectron spectroscopy (XPS) and X--ray exaction (XRD)etc aam oxide film consists mainly of ZnO, Al2O3 and Zn while a small amount of MgO, MgAl2O4 and Cu also exist in the film. The chides of MgO and MgAl2O4 are obviously concentrated on the surface of the film. In these chides, the phenomenon of an excess of metallic ions is quit evident. In addition, it has been proved that, due to the oxidizing the contents of Zn and Mg in the melt will decrease and that of Al and Cu will increase.
Key words:  Zn base alloy      Oxidation     
Received:  18 June 1998     
Service
E-mail this article
Add to citation manager
E-mail Alert
RSS
()
Articles by authors

URL: 

https://www.ams.org.cn/EN/     OR     https://www.ams.org.cn/EN/Y1998/V34/I6/621

1 中国机械工程学会铸造专业学会 铸造手册-铸造非铁合金,第3卷北京:机械工业出版社,1993:24(The Foudry Institute of Chinese Mechanical Engineering .Foundry Handbooks -Foundry Nonfeerous Alloys ,V.S. Beijing: Mechanical Industry Pres 1993: 24)
2 山下次郎,国井真澄.铸造工学,1996;(3)68:249(Jiro Yamashita, Masumi Kunni.J Jpn Foundry Soc. 1996;(3)68: 249)
3 Mahanti R K, Lal K, Sivaramakrisbnan C S, Mohanty O N, Jian K B. The Thansactions of AmericanFoundryman Society, 1992; 100: 857
4 PH1 5300 Instrument Manual . USA: Perkin—Elmer Corporation, 1989: 520
5 Wagner C D, Riggs W M, Davis L E, Mouldef J F, Muilehberg G E. Handbook of X-ray Photoelectron Spetroacopy. USA: Perkin-Elmet Corpoetatiorp Phpoical Electronic Division, 1978: 50
6 Power Diffraction File.USA:Inernational Centre for Diffraction Data ,1989:5-0669,21—1486,21—1152
7 樱并良文,小泉光惠等著,陈俊彦,王余君译.新型陶瓷-材料及应用.北京:中国建筑工业出版社,1983:77(Sakurai Yoshibumi, Koisumi Mitsuye et al、 Advanced Cermaic-materials and Applications Beijing ThePress of China Building and Construction Induaryt 1983: 77)
8 梁英教,车荫昌 无机物热力学数据手册.沈阳:东北大学出版社.1993:450—478(Liang Y J, Che Y C.Thermodynamic Data Handbook of inorganic Substances .Shenyand :NortheasternUniversity Press, 1993: 450)
9 吴清辉.表面化学与多相催化北京:化学工业出版社,1991:87(Wu QH.Surface Chemistry and heterogeneous Catahysis Beijing :Chemistry Industry Press ,,1991:87)
10 West R C, Astle M Jt Beyer W H. CRC Hondbok of Chemistry and Physica,69th Edition. USA: CRC Press, Inc. 1988: F-20
11 陈鸿海 金属腐蚀学.北京:北京理工大学出版社,1995:34(Chen H H. Metallic Corrosion .Beijing .The Press of Beijing Institute fo Technology 1995: 34)
[1] HUANG Ding, QIAO Yanxin, YANG Lanlan, WANG Jinlong, CHEN Minghui, ZHU Shenglong, WANG Fuhui. Effect of Shot Peening of Substrate Surface on Cyclic Oxidation Behavior of Sputtered Nanocrystalline Coating[J]. 金属学报, 2023, 59(5): 668-678.
[2] SHEN Zhao, WANG Zhipeng, HU Bo, LI Dejiang, ZENG Xiaoqin, DING Wenjiang. Research Progress on the Mechanisms Controlling High-Temperature Oxidation Resistance of Mg Alloys[J]. 金属学报, 2023, 59(3): 371-386.
[3] LIU Laidi, DING Biao, REN Weili, ZHONG Yunbo, WANG Hui, WANG Qiuliang. Multilayer Structure of DZ445 Ni-Based Superalloy Formed by Long Time Oxidation at High Temperature[J]. 金属学报, 2023, 59(3): 387-398.
[4] LI Xin, JIANG He, YAO Zhihao, DONG Jianxin. Theoretical Calculation and Analysis of the Effect of Oxygen Atom on the Grain Boundary of Superalloy Matrices Ni, Co and NiCr[J]. 金属学报, 2023, 59(2): 309-318.
[5] XU Wenguo, HAO Wenjiang, LI Yingju, ZHAO Qingbin, LU Bingyu, GUO Heyi, LIU Tianyu, FENG Xiaohui, YANG Yuansheng. Effects of Trace Aluminum and Titanium on High Temper-ature Oxidation Behavior of Inconel 690 Alloy[J]. 金属学报, 2023, 59(12): 1547-1558.
[6] HU Min, ZHOU Shengyu, GUO Jingyuan, HU Minghao, LI Chong, LI Huijun, WANG Zumin, LIU Yongchang. Oxidation Behavior of Micro-Regions in Multiphase Ni3Al-Based Superalloys[J]. 金属学报, 2023, 59(10): 1346-1354.
[7] JIN Xinyan, CHU Shuangjie, PENG Jun, HU Guangkui. Effect of Dew Point on Selective Oxidation and Decarburization of 0.2%C-1.5%Si-2.5%Mn High Strength Steel Sheet During Continuous Annealing[J]. 金属学报, 2023, 59(10): 1324-1334.
[8] XIE Leipeng, SUN Wenyao, CHEN Minghui, WANG Jinlong, WANG Fuhui. Effects of Processing on Microstructures and Properties of FGH4097 Superalloy[J]. 金属学报, 2022, 58(8): 992-1002.
[9] CONG Hongda, WANG Jinlong, WANG Cheng, NING Shen, GAO Ruoheng, DU Yao, CHEN Minghui, ZHU Shenglong, WANG Fuhui. A New Design Inorganic Silicate Composite Coating and Its Oxidation Behavior at High Temperature in Steam Atmosphere[J]. 金属学报, 2022, 58(8): 1083-1092.
[10] ZHAO Xiaofeng, LI Ling, ZHANG Han, LU Jie. Research Progress in High-Entropy Alloy Bond Coat Material for Thermal Barrier Coatings[J]. 金属学报, 2022, 58(4): 503-512.
[11] SU Kaixin, ZHANG Jiwang, ZHANG Yanbin, YAN Tao, LI Hang, JI Dongdong. High-Cycle Fatigue Properties and Residual Stress Relaxation Mechanism of Micro-Arc Oxidation 6082-T6 Aluminum Alloy[J]. 金属学报, 2022, 58(3): 334-344.
[12] PENG Jun, JIN Xinyan, ZHONG Yong, WANG Li. Influence of Substrate Surface Structure on the Galvanizability of Fe-16Mn-0.7C-1.5Al TWIP Steel Sheet[J]. 金属学报, 2022, 58(12): 1600-1610.
[13] CAO Chao, JIANG Chengyang, LU Jintao, CHEN Minghui, GENG Shujiang, WANG Fuhui. Corrosion Behavior of Austenitic Stainless Steel with Different Cr Contents in 700oC Coal Ash/High Sulfur Flue-Gas Environment[J]. 金属学报, 2022, 58(1): 67-74.
[14] CHEN Shenghu, RONG Lijian. Oxide Scale Formation on Ultrafine-Grained Ferritic-Martensitic Steel During Pre-Oxidation and Its Effect on the Corrosion Performance in Stagnant Liquid Pb-Bi Eutectic[J]. 金属学报, 2021, 57(8): 989-999.
[15] PI Huilong, SHI Xiaolei, XU Xingxiang. Effect of SiC-ZrC Coating Prepared by SiZr Liquid Phase Sintering on the Oxidation Resistance of C/SiC Composites[J]. 金属学报, 2021, 57(6): 791-796.
No Suggested Reading articles found!