微米级选区激光熔化316L不锈钢的拉伸力学性能
张楠1,2, 张海武2, 王淼辉1,2()
1 中机新材料研究院(郑州)有限公司 郑州 450001
2 中国机械科学研究总院集团有限公司 北京 100044
Tensile Mechanical Properties of Micro-Selective Laser Melted 316L Stainless Steel
ZHANG Nan1,2, ZHANG Haiwu2, WANG Miaohui1,2()
1 China Machinery Institute of Advanced Materials Co. Ltd., Zhengzhou 450001, China
2 China Academy of Mechanical Science and Technology Group Co. Ltd., Beijing 100044, China
引用本文:

张楠, 张海武, 王淼辉. 微米级选区激光熔化316L不锈钢的拉伸力学性能[J]. 金属学报, 2024, 60(2): 211-219.
Nan ZHANG, Haiwu ZHANG, Miaohui WANG. Tensile Mechanical Properties of Micro-Selective Laser Melted 316L Stainless Steel[J]. Acta Metall Sin, 2024, 60(2): 211-219.

全文: PDF(2840 KB)   HTML
摘要: 

为辅助理解金属材料高精密增材制造成形机理,本工作利用微米级选区激光熔化(micro-selective laser melting,M-SLM)技术制备了316L不锈钢,对其拉伸性能及断裂行为进行了研究,并对断后横向和纵向拉伸试样显微组织和断口形貌进行了表征与分析,对近断面塑性变形区的晶粒取向、晶界特征分布等进行了电子背散射衍射(EBSD)分析。结果表明:M-SLM制备316L不锈钢晶粒内部存在尺寸为100~300 nm的胞状组织结构,拉伸断口呈韧窝状,窝口直径80~500 nm,这使得316L不锈钢的横向平均抗拉强度达692.1 MPa,纵向平均断后延伸率达54.6%,明显优于传统SLM技术制备的316L不锈钢。M-SLM制备316L不锈钢在拉伸过程中奥氏体Σ3孪晶界的出现与晶粒取向有关,其在取向接近<111>的晶粒中较易出现。进一步分析指出,Σ3晶界的出现阻断了特殊晶界网络的连通性。通过基于EBSD的矩形截面法对共格Σ3 (Σ3c)和非共格Σ3 (Σ3ic)晶界进行了统计分析,显示316L横向拉伸试样近断口区的Σ3cΣ3ic晶界数量百分比分别约为43%和57%,而纵向拉伸试样近断口区的Σ3c晶界数量百分比提高至约70%。Σ3c孪晶界的增加使得总晶界能降低,是导致M-SLM制备316L不锈钢纵向拉伸强度普遍低于横向拉伸强度的原因。

关键词 微米级选区激光熔化316L不锈钢拉伸性能Σ3晶界孪晶    
Abstract

Compared with selective laser melting (SLM), the micro-SLM (M-SLM) technology offers the advantages of small spot diameter (< 20 μm), high forming precision (20-50 μm), and surface roughness (Ra) of up 1 μm, which implies that the M-SLM technology provides great potential for promotion and application in communication electronics, biomedical, and other fields in the future. In this work, 316L stainless steel was prepared using M-SLM, and its tensile properties and fracture behavior were studied. The microstructures of transverse and longitudinal tensile specimens were also investigated. In addition, the fracture morphology was characterized and analyzed, and the grain orientation and grain-boundary-characteristic distribution in the near-section plastic-deformation zone were further analyzed using electron backscatter diffraction (EBSD). The results showed that the 316L stainless steel prepared by M-SLM had a cellular structure with a size of 100-300 nm inside the grains. The tensile fracture was dimple-shaped, and the average dimple diameter was 80-500 nm, which allowed the transverse average tensile strength of the 316L stainless steel to reach 692.1 MPa, the longitudinal average elongation after fracture was 54.6%, which were obviously better than that of the 316L stainless steel prepared using traditional SLM. The appearance of austenite Σ3 twin boundaries in the stretching process of the 316L stainless steel prepared by M-SLM was related to the grain orientation, which could more likely appear in grains with an orientation close to <111>. Further analysis indicated that the appearance of Σ3 grain boundaries blocked the connectivity of the special grain-boundary network. Statistical analysis of the coherent Σ3 (Σ3c) and incoherent Σ3 (Σ3ic) grain boundaries using the EBSD-based rectangular-section method revealed that the amount percentages of Σ3c and Σ3ic in the near-fracture region of the 316L transverse tensile specimen were approximately 43% and 57%, respectively. Meanwhile, the amount percentage of Σ3c in the same region of the 316L longitudinal tensile specimen increased to approximately 70%. The increase in the coherent Σ3c twin boundary reduced the total grain-boundary energy, which explained why the longitudinal tensile strength of the 316L stainless steel prepared by M-SLM was generally lower than the transverse tensile strength.

Key wordsmicro-selective laser melting    316L stainless steel    tensile property    Σ3 boundary    twinning
收稿日期: 2022-02-14     
ZTFLH:  TG142  
基金资助:国家自然科学基金项目(51975240);北京市自然科学基金项目(2222093);中国机械科学研究总院集团技术发展基金项目(812201Q9)
通讯作者: 王淼辉,wangmh0103@163.com,主要从事金属增材制造技术研究
Corresponding author: WANG Miaohui, professor, Tel: (010)60603546, E-mail: wangmh0103@163.com
作者简介: 张 楠,男,1983年生,高级工程师,博士
图1  微米级选区激光熔化(M-SLM)制备拉伸试样尺寸示意图
图2  316L不锈钢粉末的SEM像
图3  M-SLM成形316L不锈钢的XRD谱
图4  M-SLM成形316L不锈钢横向和纵向显微组织的SEM像
图5  M-SLM成形316L不锈钢工程应力-应变曲线
DirectionRm / MPaδ / %UT / (J·cm-3)
Transverse692.132.0210.6
Longitudinal642.354.6331.9
表1  M-SLM成形316L不锈钢不同增材方向的拉伸性能
图6  M-SLM和传统SLM成形316L不锈钢拉伸力学性能比较
图7  M-SLM成形不同方向316L不锈钢拉伸断口形貌的SEM像
图8  M-SLM成形316L不锈钢横向和纵向试样拉伸断裂区微观组织EBSD分析(a, d) inverse pole figures (IPFs)(b, e) special grain boundary distribution maps(c, f) deformed metal distribution maps
图9  M-SLM成形316L不锈钢纵向试样拉伸断裂区孪晶晶粒标准取向三角图
图10  微矩形截面法判定图8b中圈圈区域Σ3晶界的示意图(a) Σ3 grain boundary(b) pole figure of {111} crystal form
No.φ / (o)TypeNo.φ / (o)Type
8b-1+4IC8e-1+8IC
8b-2-2C8e-2-1C
8b-3+6IC8e-3-2C
8b-4+2C8e-40C
8b-50C8e-5-2C
8b-6-6IC8e-6+4IC
8b-7+4IC8e-7-3C
8b-8-1C8e-8+3C
8b-9+7IC8e-9-9IC
8b-10-3C8e-10-2C
8b-11-5IC8e-11-7IC
8b-12+3C8e-12-2C
8b-13-7IC8e-13+1C
8b-14+2C8e-14-4IC
8b-15-6IC8e-15+7IC
8b-16-3C8e-16+1C
8b-17+9IC8e-17-2C
8b-18-6IC8e-18+5IC
8b-19+3C8e-19+1C
8b-20+4IC8e-20-2C
8b-21+1C8e-21-3C
8b-22-5IC8e-22+5IC
8b-23+6IC8e-23+1C
8b-24-4IC8e-240C
8b-25-1C8e-25-1C
8b-260C8e-26+2C
8b-27+7IC8e-27-2C
8b-28-5IC8e-28+3C
8b-29-6IC8e-29+1C
8b-30-2C8e-30+4IC
表2  图8b和e中Σ3晶界分析结果
1 Lan H B, Li D C, Lu B H. Micro- and nanoscale 3D printing [J]. Sci. Sin. Technol., 2015, 45: 919
doi: 10.1360/N092014-00397
1 兰红波, 李涤尘, 卢秉恒. 微纳尺度3D打印 [J]. 中国科学: 技术科学, 2015, 45: 919
2 Liu G, Zhang X F, Chen X L, et al. Additive manufacturing of structural materials [J]. Mater. Sci. Eng., 2021, R145: 100596
3 Gunasekaran J, Sevvel P, Solomon I J. Metallic materials fabrication by selective laser melting: A review [J]. Mater. Today Proc., 2020, 37: 252
4 Jin X Y, Lan L, He B, et al. A review on surface roughness of metals parts fabricated by selective laser melting [J]. Mater. Rep., 2021, 35: 3168
4 金鑫源, 兰 亮, 何 博 等. 选区激光熔化成形金属零件表面粗糙度研究进展 [J]. 材料导报, 2021, 35: 3168
5 Zhang X Z, Chen L, Zhou J, et al. Simulation and experimental studies on process parameters, microstructure and mechanical properties of selective laser melting of stainless steel 316L [J]. J. Braz. Soc. Mech. Sci. Eng., 2020, 42: 402
doi: 10.1007/s40430-020-02491-3
6 Greco S, Gutzeit K, Hotz H, et al. Selective laser melting (SLM) of AISI 316L——Impact of laser power, layer thickness, and hatch spacing on roughness, density, and microhardness at constant input energy density [J]. Int. J. Adv. Manuf. Technol., 2020, 108: 1551
doi: 10.1007/s00170-020-05510-8
7 Stoll P, Spierings A, Wegener K. Impact of a process interruption on tensile properties of SS 316L parts and hybrid parts produced with selective laser melting [J]. Int. J. Adv. Manuf. Technol., 2019, 103: 367
doi: 10.1007/s00170-019-03560-1
8 Tascioglu E, Karabulut Y, Kaynak Y. Influence of heat treatment temperature on the microstructural, mechanical, and wear behavior of 316L stainless steel fabricated by laser powder bed additive manufacturing [J]. Int. J. Adv. Manuf. Technol., 2020, 107: 1947
doi: 10.1007/s00170-020-04972-0
9 Yang X Q, Liu Y, Ye J W, et al. Enhanced mechanical properties and formability of 316L stainless steel materials 3D-printed using selective laser melting [J]. Int. J. Miner. Metall. Mater., 2019, 26: 1396
doi: 10.1007/s12613-019-1837-2
10 Yang D C, Kan X F, Gao P F, et al. Influence of porosity on mechanical and corrosion properties of SLM 316L stainless steel [J]. Appl. Phys., 2022, 128A: 51
11 Yang X, Ma W J, Ren Y J, et al. Subgrain microstructures and tensile properties of 316L stainless steel manufactured by selective laser melting [J]. J. Iron Steel Res. Int., 2021, 28: 1159
doi: 10.1007/s42243-021-00561-x
12 Shin W S, Son B, Song W S, et al. Heat treatment effect on the microstructure, mechanical properties, and wear behaviors of stainless steel 316L prepared via selective laser melting [J]. Mater. Sci. Eng., 2021, A806: 140805
13 Wang Y M, Voisin T, McKeown J T, et al. Additively manufactured hierarchical stainless steels with high strength and ductility [J]. Nat. Mater., 2018, 17: 63
doi: 10.1038/nmat5021 pmid: 29115290
14 Shamsujjoha M, Agnew S R, Fitz-Gerald J M, et al. High strength and ductility of additively manufactured 316L stainless steel explained [J]. Metall. Mater. Trans., 2018, 49A: 3011
15 Kong D C, Dong C F, Wei S L, et al. About metastable cellular structure in additively manufactured austenitic stainless steels [J]. Addit. Manuf., 2021, 38: 101804
16 Nagarajan B, Hu Z H, Song X, et al. Development of micro selective laser melting: The state of the art and future perspectives [J]. Engineering, 2019, 5: 702
doi: 10.1016/j.eng.2019.07.002
17 Bertoli U S, Wolfer A J, Matthews M J, et al. On the limitations of volumetric energy density as a design parameter for selective laser melting [J]. Mater. Des., 2017, 113: 331
doi: 10.1016/j.matdes.2016.10.037
18 Brandon D G. The structure of high-angle grain boundaries [J]. Acta Metall., 1966, 14: 1479
doi: 10.1016/0001-6160(66)90168-4
19 Elmer J W, Allen S M, Eagar T W. Microstructural development during solidification of stainless steel alloys [J]. Metall. Trans., 1989, 20A: 2117
20 Zong X W, Gao Q, Zhou H Z, et al. Effects of bulk laser energy density on anisotropy of selective laser sintered 316L stainless steel [J]. Chin. J. Lasers, 2019, 46: 0502003
20 宗学文, 高 倩, 周宏志 等. 体激光能量密度对选区激光熔化316L不锈钢各向异性的影响 [J]. 中国激光, 2019, 46: 0502003
21 Lu L, Li Z B, Bi Z Y, et al. Relationship between tension toughness and fracture toughness of low carbon low alloy steel [J]. J. Iron Steel Res., 2014, 26(6): 67
21 芦 琳, 李周波, 毕宗岳 等. 低碳低合金钢的静力韧度与断裂韧度 [J]. 钢铁研究学报, 2014, 26(6): 67
22 Gu D D, Chen H Y. Selective laser melting of high strength and toughness stainless steel parts: The roles of laser hatch style and part placement strategy [J]. Mater. Sci. Eng., 2018, A725: 419
23 Gu D D, Shi X Y, Poprawe R, et al. Material-structure-performance integrated laser-metal additive manufacturing [J]. Science, 2021, 372: eabg1487
doi: 10.1126/science.abg1487
24 Qi B, Liu Y D, Shi W T, et al. Study on overlap ratio of pulse laser selective melting forming [J]. Laser Technol., 2018, 42: 311
24 祁 斌, 刘玉德, 石文天 等. 脉冲式激光选区熔化成形搭接率的研究 [J]. 激光技术, 2018, 42: 311
25 Ma Y Y, Liu Y D, Shi W T, et al. Effect of scanning speed on forming defects and properties of selective laser melted 316L stainless steel powder [J]. Laser Optoelectr. Progr., 2019, 56: 101403
doi: 10.3788/LOP
25 马英怡, 刘玉德, 石文天 等. 扫描速度对选区激光熔化316L不锈钢粉末成形缺陷及性能的影响 [J]. 激光与光电子学进展, 2019, 56: 101403
26 Shi W T, Wang P, Liu Y D, et al. Experimental study on surface quality and process of selective laser melting forming 316L [J]. Surface Technol., 2019, 48: 257
26 石文天, 王 朋, 刘玉德 等. 选区激光熔化成形316L表面质量及工艺试验研究 [J]. 表面技术, 2019, 48: 257
27 Afkhami S, Dabiri M, Piili H, et al. Effects of manufacturing parameters and mechanical post-processing on stainless steel 316L processed by laser powder bed fusion [J]. Mater. Sci. Eng., 2021, A802: 140660
28 Kumar P, Jayaraj R, Suryawanshi J, et al. Fatigue strength of additively manufactured 316L austenitic stainless steel [J]. Acta Mater., 2020, 199: 225
doi: 10.1016/j.actamat.2020.08.033
29 Wu D J, Yu C S, Wang Q Y, et al. Synchronous-hammer-forging-assisted laser directed energy deposition additive manufacturing of high-performance 316L samples [J]. J. Mater. Process. Technol., 2022, 307: 117695
doi: 10.1016/j.jmatprotec.2022.117695
30 Matthews M J, Guss G, Khairallah S A, et al. Denudation of metal powder layers in laser powder bed fusion processes [J]. Acta Mater., 2016, 114: 33
doi: 10.1016/j.actamat.2016.05.017
31 Yu C F, Zhao C C, Zhang Z F, et al. Tensile properties of selective laser melted 316L stainless steel [J]. Acta Metall. Sin., 2020, 56: 683
doi: 10.11900/0412.1961.2019.00278
31 余晨帆, 赵聪聪, 张哲峰 等. 选区激光熔化316L不锈钢的拉伸性能 [J]. 金属学报, 2020, 56: 683
doi: 10.11900/0412.1961.2019.00278
32 Gutierrez-Urrutia I, Zaefferer S, Raabe D. The effect of grain size and grain orientation on deformation twinning in a Fe-22wt.%Mn-0.6wt.%C TWIP steel [J]. Mater. Sci. Eng., 2010, A527: 3552
33 Sun S J, Tian Y Z, Lin H R, et al. Transition of twinning behavior in CoCrFeMnNi high entropy alloy with grain refinement [J]. Mater. Sci. Eng., 2018, A712: 603
34 de Campos M F, Loureiro S A, Rodrigues D, et al. Estimative of the stacking fault energy for a FeNi(50/50) alloy and a 316L stainless steel [J]. Mater. Sci. Forum, 2008, 591-593: 3
doi: 10.4028/www.scientific.net/MSF.591-593
[1] 赵鹏, 谢光, 段慧超, 张健, 杜奎. 两种高代次镍基单晶高温合金热机械疲劳中的再结晶行为[J]. 金属学报, 2023, 59(9): 1221-1229.
[2] 白佳铭, 刘建涛, 贾建, 张义文. WTa型粉末高温合金的蠕变性能及溶质原子偏聚[J]. 金属学报, 2023, 59(9): 1230-1242.
[3] 邵晓宏, 彭珍珍, 靳千千, 马秀良. 镁合金LPSO/SFs结构间{10ˉ12}孪晶交汇机制的原子尺度研究[J]. 金属学报, 2023, 59(4): 556-566.
[4] 万涛, 程钊, 卢磊. 组元占比对层状纳米孪晶Cu力学行为的影响[J]. 金属学报, 2023, 59(4): 567-576.
[5] 王迪, 贺莉丽, 王栋, 王莉, 张思倩, 董加胜, 陈立佳, 张健. Pt-Al涂层对DD413合金高温拉伸性能的影响[J]. 金属学报, 2023, 59(3): 424-434.
[6] 孙腾腾, 王洪泽, 吴一, 汪明亮, 王浩伟. 原位自生2%TiB2 颗粒对2024Al增材制造合金组织和力学性能的影响[J]. 金属学报, 2023, 59(1): 169-179.
[7] 高栋, 周宇, 于泽, 桑宝光. 液氮温度下纯Ti动态塑性变形中的孪晶变体选择[J]. 金属学报, 2022, 58(9): 1141-1149.
[8] 卢磊, 赵怀智. 异质纳米结构金属强化韧化机理研究进展[J]. 金属学报, 2022, 58(11): 1360-1370.
[9] 潘庆松, 崔方, 陶乃镕, 卢磊. 纳米孪晶强化304奥氏体不锈钢的应变控制疲劳行为[J]. 金属学报, 2022, 58(1): 45-53.
[10] 戴进财, 闵小华, 周克松, 姚凯, 王伟强. 预变形与等温时效耦合作用下Ti-10Mo-1Fe/3Fe层状合金的力学性能[J]. 金属学报, 2021, 57(6): 767-779.
[11] 温斌, 田永君. 纳米孪晶金属和纳米孪晶共价材料的力学行为[J]. 金属学报, 2021, 57(11): 1380-1395.
[12] 刘先锋, 刘冬, 刘仁慈, 崔玉友, 杨锐. Ti-43.5Al-4Nb-1Mo-0.1B合金的包套热挤压组织与拉伸性能[J]. 金属学报, 2020, 56(7): 979-987.
[13] 余晨帆, 赵聪聪, 张哲峰, 刘伟. 选区激光熔化316L不锈钢的拉伸性能[J]. 金属学报, 2020, 56(5): 683-692.
[14] 李源才, 江五贵, 周宇. 纳米孔洞对单晶/多晶Ni复合体拉伸性能的影响[J]. 金属学报, 2020, 56(5): 776-784.
[15] 王希,刘仁慈,曹如心,贾清,崔玉友,杨锐. 冷却速率对β凝固γ-TiAl合金硼化物和室温拉伸性能的影响[J]. 金属学报, 2020, 56(2): 203-211.