Please wait a minute...
金属学报  2018, Vol. 54 Issue (7): 1077-1086    DOI: 10.11900/0412.1961.2017.00426
  本期目录 | 过刊浏览 |
倒装芯片无铅凸点β-Sn晶粒取向与电迁移交互作用
黄明亮(), 孙洪羽
大连理工大学材料科学与工程学院 先进连接技术辽宁省重点实验室 大连 116024
Interaction Between β-Sn Grain Orientation and Electromigration Behavior in Flip-Chip Lead-Free Solder Bumps
Mingliang HUANG(), Hongyu SUN
Key Laboratory of Liaoning Advanced Welding and Joining Technology, School of Materials Science and Engineering, Dalian University of Technology, Dalian 116024, China
引用本文:

黄明亮, 孙洪羽. 倒装芯片无铅凸点β-Sn晶粒取向与电迁移交互作用[J]. 金属学报, 2018, 54(7): 1077-1086.
Mingliang HUANG, Hongyu SUN. Interaction Between β-Sn Grain Orientation and Electromigration Behavior in Flip-Chip Lead-Free Solder Bumps[J]. Acta Metall Sin, 2018, 54(7): 1077-1086.

全文: PDF(8515 KB)   HTML
摘要: 

采用原位电迁移实验研究了在150 ℃、1.0×104 A/cm2条件下倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点中β-Sn晶粒取向对金属间化合物(IMC)的聚集析出机制、阴极Ni芯片侧(UBM)溶解行为、电迁移失效机制以及电迁移驱动下β-Sn晶粒的旋转滑移机制的影响。原位观察发现,电迁移过程中(Ni, Cu)3Sn4类型IMC在凸点中仅沿着β-Sn晶粒的c轴方向析出,且倾向于在θ角(β-Sn晶粒的c轴与电子流动方向之间的夹角)较小的晶粒内析出;同时,阳极附近观察到β-Sn挤出现象,即凸点出现应力松弛。建立了阴极Ni UBM溶解量与β-Sn晶粒取向的关系模型:β-Sn晶粒取向决定阴极Ni UBM的溶解量,即当θ角很小时,Ni UBM会出现明显溶解;当θ角增大时,Ni UBM的溶解受到抑制,该模型与实验值基本吻合。电迁移导致β-Sn晶粒发生旋转滑移,认为是由于不同取向的相邻β-Sn晶粒中电迁移导致的空位通量不同,从而导致阳极晶界处于空位的过饱和,阴极晶界处于空位的未饱和状态,并促使空位沿着晶界出入于自由表面,最终在垂直方向上会产生空位梯度,由沿晶界的空位梯度对应的应力梯度产生的力矩使β-Sn晶粒发生旋转滑移。

关键词 : 电迁移,  β-Sn;,  各向异性,  阴极溶解,  IMC析出,  晶粒旋转    
Abstract:

With the increasing demands for miniaturization, the electromigration (EM)-induced failure by diffusion anisotropy in β-Sn is expected to be more serious than that induced by local current crowding effect, especially with the downsizing of solder bumps. In this work, the effects of Sn grain orientation on intermetallic compound (IMC) precipitation, dissolution of Ni under bump metallurgy (UBM) at the cathode, EM failure mechanism as well as the EM-induced β-Sn grain rotation in Ni/Sn-3.0Ag-0.5Cu/Ni-P flip-chip interconnects undergoing solid-solid EM under a current density of 1.0×104 A/cm2 at 150 ℃ were in situ studied. (Ni, Cu)3Sn4-type IMCs precipitated in these β-Sn grains with a small angle θ (between the c-axis of Sn grain and electron flow direction), i.e., along the c-axis of β-Sn grains. Stress relaxation, squeezing β-Sn whiskers near the anode, was also observed during EM. A mathematical model on the relationship between the dissolution of Ni UBM and β-Sn grain orientation was proposed: when the c-axis of β-Sn grain is parallel to the electron flow direction, excessive dissolution of the cathode Ni UBM occurred due to the large diffusivity of Ni along the c-axis; when the c-axis of β-Sn grain is perpendicular to the electron flow direction, no evident dissolution of cathode Ni UBM occurred. The proposed model agreed well with the experimental results. EM-induced β-Sn grain rotation was attributed to the different vacancy fluxes caused by EM between adjacent grains of various grain orientation, when vacancies reached supersaturation and undersaturation at the interfaces of the anode and the cathode, respectively. Vacancy fluxes went through free surface along the interface, resulting in a normal vacancy concentration gradient. Accordingly, stress gradient produces a torque to rotate the β-Sn grain.

Key words: electromigration    β-Sn;    anisotropy    cathode dissolution    IMC precipitation    grain rotation
收稿日期: 2017-10-13     
ZTFLH:  TN405  
基金资助:国家自然科学基金项目Nos.51475072、51511140289和51671046,中央高校基本科研业务费项目No.DUT17ZD202
作者简介:

作者简介 黄明亮,男,1970年生,教授,博士

图1  倒装芯片Ni/Sn-3.0Ag-0.5Cu/ENEPIG无铅凸点结构示意图
图2  倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点回流后初始微观形貌
图3  1号倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点在150 ℃、1.0×104 A/cm2条件下原位电迁移不同时间后的微观形貌及沿轴向的EBSD取向分布
图4  2号倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点在150 ℃、1.0×104 A/cm2条件下原位电迁移不同时间后的微观形貌及沿RD方向的EBSD取向分布
图5  3号倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点在150 ℃、1.0×104 A/cm2条件下原位电迁移不同时间后的微观形貌及沿RD方向的EBSD取向分布
图6  4号倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点在150 ℃、1.0×104 A/cm2条件下原位电迁移不同时间后的微观形貌及沿RD方向的EBSD取向分布
图7  5号倒装芯片Ni/Sn-3.0Ag-0.5Cu/Ni-P无铅凸点在150 ℃、1.0×104 A/cm2条件下原位电迁移不同时间后的微观形貌及沿RD方向的EBSD取向分布
  
Axis ρ γ E D (150 ℃) / (cm2s-1) DT (150 ℃)
μΩcm 10-6 ℃-1 GPa Ag Cu Ni m2s-1
a 13.25 15.45 22.9 5.60×10-11 1.99×10-7 3.85×10-9 8.70×10-13
c 20.27 30.50 68.9 3.13×10-9 8.57×10-6 1.17×10-4 4.71×10-13
表1  β-Sn的各向异性参数[8,9,10]
Parameter Valne Unit
Z*[23] 3.5 -
CNi 1.858×1024 atomsm-3
T 423 K
i 1.0×108 Am-2
ρSn 1.18×10-7 Ωm
Ω 6.6×10-6 m3mol-1
l 1.0 μm
δ 0.0125 μm
表2  计算用材料参数
图9  阴极Ni UBM消耗和q角的函数关系
图10  倒装芯片Sn-3.0Ag-0.5Cu无铅凸点中电迁移致晶粒旋转示意图
[1] Jung Y, Yu J.Electromigration induced kirkendall void growth in Sn-3.5Ag/Cu solder joints[J]. J. Appl. Phys., 2014, 115: 083708
[2] Huang M L, Zhou S M, Chen L D.Electromigration-induced interfacial reactions in Cu/Sn/Electroless Ni-P solder interconnects[J]. J. Electron. Mater., 2012, 41: 730
[3] Chen L D, Huang M L, Zhou S M.Effect of electromigration on intermetallic compound formation in line-type Cu/Sn/Cu interconnect[J]. J. Alloys Compd., 2010, 504: 535
[4] Chen C, Tong H M, Tu K N.Electromigration and thermomigration in Pb-free flip-chip solder joints[J]. Annu. Rev. Mater. Res., 2010, 40: 531
[5] Huang M L, Ye S, Zhao N.Current-induced interfacial reactions in Ni/Sn-3Ag-0.5Cu/Au/Pd(P)/Ni-P flip chip interconnect[J]. J. Mater. Res., 2011, 26: 3009
[6] Kim K S, Huh S H, Suganuma K.Effects of intermetallic compounds on properties of Sn-Ag-Cu lead-free soldered joints[J]. J. Alloys Compd., 2003, 352: 226
[7] Zhang Z J.Liquid-solid electromigration behavior and mechanism of micro interconnect [D]. Dalian: Dalian University of Technology, 2016
[8] Dyson B F, Anthony T R, Turnbull D.Interstitial diffusion of copper in tin[J]. J. Appl. Phys., 1967, 37: 3408
[9] Yeh D C, Huntington H B.Extreme fast-diffusion system: Nickel in single-crystal tin[J]. Phys. Rev. Lett., 1984, 53: 1469
[10] Huang F H, Huntington H B.Diffusion of Sb124, Cd109, Sn113, and Zn65 in tin[J]. Phys. Rev., 1974, 9B: 1479
[11] Lu M H, Shih D Y, Lauro P, et al.Effect of Sn grain orientation on electromigration degradation mechanism in high Sn-based Pb-free solders[J]. Appl. Phys. Lett., 2008, 92: 211909
[12] Huang M L, Zhang Z J, Zhao N, et al.In situ study on reverse polarity effect in Cu/Sn-9Zn/Ni interconnect undergoing liquid-solid electromigration[J]. J. Alloys Compd., 2015, 619: 667
[13] Huang M L, Zhao J F, Zhang Z J, et al.Dominant effect of high anisotropy in β-Sn grain on electromigration-induced failure mechanism in Sn3.0Ag-0.5Cu interconnect[J]. J. Alloys Compd., 2016, 678: 370
[14] Harris K E, Singh V V, King A H.Grain rotation in thin films of gold[J]. Acta Mater., 1998, 46: 2623
[15] Moldovan D, Yamakov V, Wolf D, et al.Scaling behavior of grain-rotation-induced grain growth[J]. Phys. Rev. Lett., 2002, 89: 206101
[16] Lloyd J R.Electromigration induced resistance decrease in Sn conductors[J]. J. Appl. Phys., 2003, 94: 6483
[17] Wu A T, Gusak A M, Tu K N, et al.Electromigration-induced grain rotation in anisotropic conducting beta tin[J]. Appl. Phys. Lett., 2005, 86: 241902
[18] Wu A T, Hsieh Y C.Direct observation and kinetic analysis of grain rotation in anisotropic tin under electromigration[J]. Appl. Phys. Lett., 2008, 92: 121921
[19] Huntington H B, Grone A R.Current-induced marker motion in gold wires[J]. J. Phys. Chem. Solids, 1961, 20: 76
[20] Shi J H, Huntington H B.Electromigration of gold and silver in single crystal tin[J]. J. Phys. Chem. Solids, 1987, 48: 693
[21] Prakash K H, Sritharan T.Interface reaction between copper and molten tin-lead solders[J]. Acta Mater., 2001, 49: 2481
[22] Liu C Y, Ke L, Chuang Y C, et al.Study of electromigration-induced Cu consumption in the flip-chip Sn/Cu solder bumps[J]. J. Appl. Phys., 2006, 100: 083702
[23] Linares X, Kinney C, Lee K O, et al.The Influence of Sn orientation on intermetallic compound evolution in idealized Sn-Ag-Cu 305 interconnects: An electron backscatter diffraction study of electromigration[J]. J. Electron. Mater., 2014, 43: 43
[24] Huntington H B.Diffusion in Solids: Recent Developments [M]. New York: Academic Press, 1975: 303
[25] Huang M L, Zhang Z J, Zhao N, et al.A synchrotron radiation real-time in situ imaging study on the reverse polarity effect in Cu/Sn-9Zn/Cu interconnect during liquid-solid electromigration[J]. Scr. Mater., 2013, 68: 853
[1] 张子轩, 于金江, 刘金来. 镍基单晶高温合金DD432的持久性能各向异性[J]. 金属学报, 2023, 59(12): 1559-1567.
[2] 葛进国, 卢照, 何思亮, 孙妍, 殷硕. 电弧熔丝增材制造2Cr13合金组织与性能各向异性行为[J]. 金属学报, 2023, 59(1): 157-168.
[3] 高钰璧, 丁雨田, 李海峰, 董洪标, 张瑞尧, 李军, 罗全顺. 变形速率对GH3625合金弹-塑性变形行为的影响[J]. 金属学报, 2022, 58(5): 695-708.
[4] 卢磊, 赵怀智. 异质纳米结构金属强化韧化机理研究进展[J]. 金属学报, 2022, 58(11): 1360-1370.
[5] 王迪, 黄锦辉, 谭超林, 杨永强. 激光增材制造过程中循环热输入对组织和性能的影响[J]. 金属学报, 2022, 58(10): 1221-1235.
[6] 毕胜, 李泽琛, 孙海霞, 宋保永, 刘振宇, 肖伯律, 马宗义. 高能球磨结合粉末冶金法制备碳纳米管增强7055Al复合材料的微观组织和力学性能[J]. 金属学报, 2021, 57(1): 71-81.
[7] 刘金来, 叶荔华, 周亦胄, 李金国, 孙晓峰. 一种单晶高温合金的弹性性能的各向异性[J]. 金属学报, 2020, 56(6): 855-862.
[8] 张志杰, 黄明亮. 原位研究Cu/Sn-37Pb/Cu微焊点液-固电迁移行为[J]. 金属学报, 2020, 56(10): 1386-1392.
[9] 胡斌,李树索,裴延玲,宫声凯,徐惠彬. <111>取向小角偏离对一种镍基单晶高温合金蠕变性能的影响[J]. 金属学报, 2019, 55(9): 1204-1210.
[10] 王莉,何禹锋,申健,郑伟,楼琅洪,张健. 第二取向对第三代单晶高温合金热疲劳过程中冷却孔孔周氧化行为的影响研究[J]. 金属学报, 2019, 55(11): 1417-1426.
[11] 何贤美, 童六牛, 高成, 王毅超. Nd含量对磁控溅射Si(111)/Cr/Nd-Co/Cr薄膜结构与磁性的影响[J]. 金属学报, 2019, 55(10): 1349-1358.
[12] 马晓琴, 詹清峰, 李金财, 刘青芳, 王保敏, 李润伟. 倾斜溅射对CoFeB薄膜条纹磁畴结构与磁各向异性的影响[J]. 金属学报, 2018, 54(9): 1281-1288.
[13] 王强, 董蒙, 孙金妹, 刘铁, 苑轶. 强磁场下合金凝固过程控制及功能材料制备[J]. 金属学报, 2018, 54(5): 742-756.
[14] 李旭东, 毛萍莉, 刘晏宇, 刘正, 王志, 王峰. 高应变速率下Mg-3Zn-1Y镁合金的各向异性及变形机制[J]. 金属学报, 2018, 54(4): 557-565.
[15] 季培蓓, 周立初, 周雪峰, 方峰, 蒋建清. 冷拉拔珠光体钢丝的力学性能各向异性研究[J]. 金属学报, 2018, 54(4): 494-500.