Please wait a minute...
金属学报  2017, Vol. 53 Issue (4): 423-432    DOI: 10.11900/0412.1961.2016.00291
  本期目录 | 过刊浏览 |
Ru对一种高Cr镍基单晶高温合金凝固组织的影响
宁礼奎(),佟健,刘恩泽,谭政,纪慧思,郑志
中国科学院金属研究所 沈阳 110016
Effect of Ru on the Solidification Microstructure of a Ni-Based Single Crystal Superalloy with High Cr Content
Likui NING(),Jian TONG,Enze LIU,Zheng TAN,Huisi JI,Zhi ZHENG
Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
引用本文:

宁礼奎,佟健,刘恩泽,谭政,纪慧思,郑志. Ru对一种高Cr镍基单晶高温合金凝固组织的影响[J]. 金属学报, 2017, 53(4): 423-432.
Likui NING, Jian TONG, Enze LIU, Zheng TAN, Huisi JI, Zhi ZHENG. Effect of Ru on the Solidification Microstructure of a Ni-Based Single Crystal Superalloy with High Cr Content[J]. Acta Metall Sin, 2017, 53(4): 423-432.

全文: PDF(10721 KB)   HTML
摘要: 

以一种新型高Cr镍基单晶高温合金为基础,调整Ru的添加量,通过对3种不同Ru含量合金铸态组织的观察,研究了Ru对合金相析出特征与元素分布规律的影响。结果表明,随着Ru含量(0、1.5%、3%,质量分数)的增加,合金一次枝晶间距与二次枝晶间距逐渐减小,(γ+γ′)共晶含量先增后降,γ′相尺寸逐渐变小;3%的Ru添加使合金凝固组织中析出β-NiAl相,该相除Ni、Al基本组成元素外,还包含一定量的Cr、Co和Ru;Ru对合金中其它元素具有典型的“逆分配”作用,β-NiAl相的析出降低了Ru对其它元素“逆分配”的影响程度;Ru提高了正偏析元素Ta、Al和负偏析元素Re的偏析程度,降低了正偏析元素Mo、Cr的偏析程度。

关键词 : 单晶高温合金,  Ru,  β-NiAl相,  逆分配,  偏析    
Abstract:

Ni-based single crystal superalloys have been widely used in manufacturing the critical components of aero-engines, such as turbine blades and vanes. Improvements in phase stability on the addition of Ru are well known in the field of Ni-based superalloy development. Cr is beneficial to hot co-rrosion resistance of Ni-based superalloys. Generally, superalloys which used under easy corrosion conditions should contain high levels of Cr. Early researches about the influence of Ru on solidification microstructures in Ni-based single crystal alloys are mostly focused on low-Cr systerms (<6%). Since Cr has complex interactions with Ru, it is meanful to study the effects of Ru on solidification microstructures in high-Cr (>10%) Ni-based single crystal superalloy systems. The materials used in this work are Ni-based single crystal superalloy with high Cr content. Three superalloys by changing Ru addition (0, 1.5%, 3%, mass fraction) were designed. By observing the as-cast structure, the effect of Ru on the elements distribution and the precipitation characters of different phases in these alloys were studied. It is found that as the Ru content increases, the primary and secondary dendrite arm spacings decrease gradually; the volume fraction of (γ+γ′) eutectic increases firstly and then decreases; the γ′ size is reduced progressively. The addition of 3%Ru leads to the formation of β-NiAl phase, which contain a certain amount of Cr, Co and Ru except the basic elements Ni and Al. The typical "reverse partitioning" of other alloying elements is exhibited with the addition of Ru, while the formation of β-NiAl phase can reduce the "reverse partitioning" of other alloying elements. The addition of Ru could enhance the segregation of positive segregation elements Ta, Al and negative segregation element Re while reduce the segregation of positive segregation elements Mo and Cr.

Key words: single crystal superalloy    Ru    β-NiAl phase    reverse partitioning    segregation
收稿日期: 2016-07-08     
基金资助:国家自然科学基金项目 No.51501193
图1  3种不同Ru含量合金的铸态组织
图2  Ru含量与枝晶间距的关系
图3  3种不同含Ru量合金的升温DSC曲线
图4  3种不同含Ru量合金的典型铸态SEM像
图5  1.5Ru合金中板状共晶形貌及EDS分析
图6  3Ru合金中新相的形貌及其EDS分析
图7  3Ru合金中新相TEM像和SAED谱
Alloy TS TL ΔT0
0Ru 1334 1381 47
1.5Ru 1336 1381 45
3Ru 1335 1380 45
表1  3种不同Ru含量的合金在DSC升温曲线上获得的相变温度
图8  3Ru合金中β-NiAl相的SEM像及元素面分布
图9  3种不同Ru含量合金的铸态γ'相形貌
Alloy Eutectic β-NiAl Eutectic+β-NiAl
0Ru 0.45 - 0.45
1.5Ru 0.75 - 0.75
3Ru 0.39 0.99 1.38
表2  3种不同Ru含量合金中(γ+γ')共晶和β-NiAl相的体积分数
Alloy Re Mo Ru W Cr Co Al Ta Ni
0Ru 0.260 0.574 - 2.073 6.378 6.698 7.889 10.371 65.757
1.5Ru 0.361 0.640 1.264 2.208 5.619 6.663 7.667 11.937 63.641
3Ru 0.576 0.951 2.507 2.623 8.238 7.442 6.883 10.966 59.814
表3  3种合金中(γ+γ')共晶相成分的比较
图10  3种不同Ru含量合金中各元素在γ /γ'相中的分配比
图11  3种不同Ru含量合金中各元素的偏析系数K
[1] Giamei A F, Anton D L.Rhenium additions to a Ni-base superalloy: Effects on microstructure[J]. Metall. Trans., 1985, 16A: 1997
[2] Murakami T H H, Honma T, Koizumi Y, et al. Distribution of platinum group metals in Ni-base single-crystal superalloys [A]. Superalloys 2000[C]. Warrendale, PA: TMS, 2000: 747
[3] Yeh A C, Rae C M F, Tin S. High temperature creep of Ru-bearing Ni-base single crystal superalloys [A]. Superalloys 2004[C]. Warrendale, PA: TMS, 2004: 677
[4] Epishin A, Link T.Mechanisms of high temperature creep of nickel-base superalloys under low applied stress [A]. Superalloys 2004[C]. Warrendale, PA: TMS, 2004: 137
[5] Collins H E.The effect of thermal exposure on the microstructure and mechanical properties of nickel-base superalloys[J]. Metall. Trans., 1974, 5: 189
[6] Austin C M,O'Hara K S, Darolia R, et al. New nickel base super-alloy-useful for gas turbine engine single crystal air foil [P]. US Pat, 5151249-A, 1992
[7] Rea C M F, Karunaratne M S A, Small C J, et al. Topologically close packed phases in an experimental rhenium-containing single crystal superalloy [A]. Superalloys 2000[C]. Warrendale, PA: TMS, 2000: 767
[8] Rea C M F, Reed R C. The precipitation of topologically close-packed phases in rhenium-containing superalloys[J]. Acta Mater., 2001, 49: 4113
[9] Tin S, Pollock T M.Phase instabilities and carbon additions in single-crystal nickel-base superalloys[J]. Mater. Sci. Eng., 2003, A348: 111
[10] Lavigne O, Ramusat C, Drawin S, et al.Relationships between microstructural instabilities and mechanical behaviour in new generation nickel-based single crystal superalloys [A]. Superalloys 2004[C]. Warrendale, PA: TMS, 2004: 667
[11] O'Hara K S,Walston W S, Ross E W, et al. Nickel base superalloy and article [P]. US Pat, 5482789-A, 1996
[12] Walston S, Cetel A, MacKay R, et al. Joint development of a fourth generation single crystal superalloy [A]. Superalloys 2004[C]. Warrendale, PA: TMS, 2004: 15
[13] Sato A, Harada H, Yokokawa T, et al.The effects of ruthenium on the phase stability of fourth generation Ni-base single crystal superalloys[J]. Scr. Mater., 2006, 54: 1679
[14] Hobbs R A, Zhang L, Rae C M F, et al. Mechanisms of topologically close-packed phase suppression in an experimental ruthenium-bearing single-crystal nickel-base superalloy at 1100 ℃[J]. Metall. Mater. Trans., 2008, 39A: 1014
[15] Feng Q, Nandy T K, Tin S, et al.Solidification of high-refractory ruthenium-containing superalloys[J]. Acta Mater., 2003, 51: 269
[16] Hobbs R A, Tin S, Rae C M F, et al. Solidification characteristics of advanced nickel-base single crystal superalloys [A]. Super-alloys 2004[C]. Warrendale, PA: TMS, 2004: 819
[17] Kearsey R M, Beddoes J C, Jaansalu K M, et al.The effects of Re, W and Ru on microsegregation behaviour in single crystal super-alloy systems [A]. Superalloys 2004[C]. Warrendale, PA: TMS, 2004: 801
[18] Feng Q, Carroll L J, Pollock T M.Soldification segregation in ruthenium-containing nickel-base superalloys[J]. Metall. Mater. Trans., 2006, 37A: 1949
[19] Heckl A, Neumeier S, Goken M, et al.The effect of Re and Ru on γ/γ' microstructure, γ-solid solution strengthening and creep strength in nickel-base superalloys[J]. Mater. Sci. Eng., 2011, A528: 3435
[20] Jin T.Role of ruthenium in Ni-based single crystal superalloys [D]. Shenyang: Institute of Metal Research, Chinese Academy of Science, 2009
[20] (金涛. 钌在镍基单晶高温合金中的作用 [D]. 沈阳: 中国科学院金属研究所, 2009)
[21] Liu G, Liu L, Zhao X B, et al.Effects of Re and Ru on the solidification characteristics of nickel-base single-crystal superalloys[J]. Metall. Mater. Trans., 2011, 42A: 2733
[22] Caldwell E C, Fela F J, Fuchs G E.Segregation of elements in high refractory content single crystal nickel based superalloys [A]. Superalloys 2004[C]. Warrendale, PA: TMS, 2004: 811
[23] Kurz W, Fisher D J.Fundamentals of Solidification[M]. Aedermannsdorf, Switzerland: Trans Tech Pub, 1998: 247
[24] Volek A, Pyczak F, Singer R F, et al.Partitioning of Re between γ and γ' phase in nickel-base superalloys[J]. Scr. Mater., 2005, 52: 141
[25] Blavette D, Caron P, Khan T.An atom-probe study of some fine-scale microstructural features in Ni-based single crystal super-alloys [A]. Superalloys 1988[C]. Warrendale, PA: TMS, 1988: 305
[26] Giamei A F, Anton D L.Rhenium additions to a Ni-base super-alloy: Effects on microstructure[J]. Metall. Mater. Trans., 1985, 16A: 1997
[27] Guan X R.Investigation of effects of Ti, Cr and Re on microstructure and performance of Ni-based superalloy [D]. Shenyang: Northeastern University, 2010
[27] (管秀荣. Ti, Cr, Re对镍基高温合金组织及性能影响研究 [D]. 沈阳: 东北大学, 2010)
[28] Kearsey R M, Beddoes J C, Jones P, et al.Compositional design considerations for microsegregation in single crystal superalloy systems[J]. Intermetallics, 2004, 12: 903
[1] 卢楠楠, 郭以沫, 杨树林, 梁静静, 周亦胄, 孙晓峰, 李金国. 激光增材修复单晶高温合金的热裂纹形成机制[J]. 金属学报, 2023, 59(9): 1243-1252.
[2] 李嘉荣, 董建民, 韩梅, 刘世忠. 吹砂对DD6单晶高温合金表面完整性和高周疲劳强度的影响[J]. 金属学报, 2023, 59(9): 1201-1208.
[3] 张健, 王莉, 谢光, 王栋, 申健, 卢玉章, 黄亚奇, 李亚微. 镍基单晶高温合金的研发进展[J]. 金属学报, 2023, 59(9): 1109-1124.
[4] 赵鹏, 谢光, 段慧超, 张健, 杜奎. 两种高代次镍基单晶高温合金热机械疲劳中的再结晶行为[J]. 金属学报, 2023, 59(9): 1221-1229.
[5] 常松涛, 张芳, 沙玉辉, 左良. 偏析干预下体心立方金属再结晶织构竞争[J]. 金属学报, 2023, 59(8): 1065-1074.
[6] 刘继浩, 周健, 武会宾, 马党参, 徐辉霞, 马志俊. 喷射成形M3高速钢偏析成因及凝固机理[J]. 金属学报, 2023, 59(5): 599-610.
[7] 王迪, 贺莉丽, 王栋, 王莉, 张思倩, 董加胜, 陈立佳, 张健. Pt-Al涂层对DD413合金高温拉伸性能的影响[J]. 金属学报, 2023, 59(3): 424-434.
[8] 张子轩, 于金江, 刘金来. 镍基单晶高温合金DD432的持久性能各向异性[J]. 金属学报, 2023, 59(12): 1559-1567.
[9] 张利民, 李宁, 朱龙飞, 殷鹏飞, 王建元, 吴宏景. 交流电脉冲对过共晶Al-Si合金中初生Si相偏析的作用机制[J]. 金属学报, 2023, 59(12): 1624-1632.
[10] 苏震奇, 张丛江, 袁笑坦, 胡兴金, 芦可可, 任维丽, 丁彪, 郑天祥, 沈喆, 钟云波, 王晖, 王秋良. 纵向静磁场下单晶高温合金定向凝固籽晶回熔界面杂晶的形成与演化[J]. 金属学报, 2023, 59(12): 1568-1580.
[11] 陈学双, 黄兴民, 刘俊杰, 吕超, 张娟. 一种含富锰偏析带的热轧临界退火中锰钢的组织调控及强化机制[J]. 金属学报, 2023, 59(11): 1448-1456.
[12] 郭东伟, 郭坤辉, 张福利, 张飞, 曹江海, 侯自兵. 基于二次枝晶间距变化特征的连铸方坯CET位置判断新方法[J]. 金属学报, 2022, 58(6): 827-836.
[13] 李亚敏, 张瑶瑶, 赵旺, 周生睿, 刘洪军. Cu对Inconel 718合金Nb偏析影响机理的第一性原理研究[J]. 金属学报, 2022, 58(2): 241-249.
[14] 李文文, 陈波, 熊华平, 尚泳来, 毛唯, 程耀永. 第二代单晶高温合金DD6高性能钎焊接头的组织及力学性能[J]. 金属学报, 2021, 57(8): 959-966.
[15] 冯苗苗, 张红伟, 邵景霞, 李铁, 雷洪, 王强. 耦合热力学相变路径预测Fe-C包晶合金宏观偏析[J]. 金属学报, 2021, 57(8): 1057-1072.