金属学报  2024, Vol. 60 Issue (8): 1064-1078    DOI: 10.11900/0412.1961.2024.00054
  研究论文 本期目录 | 过刊浏览 |
焊前预处理对钛合金厚板焊接残余应力的影响
周牧1,2, 王倩2, 王延绪3(), 翟梓融4, 何伦华5,6, 李昺3, 马英杰1,2(), 雷家峰1,2, 杨锐1,2
1 中国科学技术大学 材料科学与工程学院 沈阳 110016
2 中国科学院金属研究所 师昌绪先进材料创新中心 沈阳 110016
3 中国科学院金属研究所 沈阳材料科学国家研究中心 沈阳 110016
4 上海科技大学 智造系统工程中心 上海 201210
5 散裂中子源科学中心 东莞 523803
6 中国科学院物理研究所 北京国家凝聚态物理学实验室 北京 100190
Effect of Prewelding Pretreatment on Welding Residual Stress of Titanium Alloy Thick Plate
ZHOU Mu1,2, WANG Qian2, WANG Yanxu3(), ZHAI Zirong4, HE Lunhua5,6, LI Bing3, MA Yingjie1,2(), LEI Jiafeng1,2, YANG Rui1,2
1 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
2 Shi -changxu Innovation Center for Advanced Materials, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
3 Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
4 Center for Adaptive System Engineering, ShanghaiTech University, Shanghai 201210, China
5 Spallation Neutron Source Science Center, Dongguan 523803, China
6 Beijing National Laboratory for Condensed Matter Physics, Institute of Physics, Chinese Academy of Sciences, Beijing 100190, China
引用本文:

周牧, 王倩, 王延绪, 翟梓融, 何伦华, 李昺, 马英杰, 雷家峰, 杨锐. 焊前预处理对钛合金厚板焊接残余应力的影响[J]. 金属学报, 2024, 60(8): 1064-1078.
Mu ZHOU, Qian WANG, Yanxu WANG, Zirong ZHAI, Lunhua HE, Bing LI, Yingjie MA, Jiafeng LEI, Rui YANG. Effect of Prewelding Pretreatment on Welding Residual Stress of Titanium Alloy Thick Plate[J]. Acta Metall Sin, 2024, 60(8): 1064-1078.

全文: PDF(5883 KB)   HTML
摘要: 

焊接残余应力是影响焊接成型及焊接部件服役的重要因素。为了优化焊接工艺和焊接接头微观结构,有效地减小焊接残余应力,本工作研究了焊前预处理工艺对电子束焊接钛合金厚板焊接接头组织、性能和残余应力的影响机制。对不同预处理工艺制备的钛合金焊接接头进行组织形貌表征,发现焊前预热显著增宽了焊接接头的熔合区和热影响区,粗化了两区域内的α片层,提高了焊接接头的强韧性匹配。采用中子衍射法、深孔法和轮廓法检测钛合金厚板电子束焊接头残余应力,对3种方法的检测结果进行对比分析,获得了焊接接头不同区域沿不同方向的残余应力分布。另外,对比了2种预热工艺焊接接头采用深孔法获得的残余应力结果,发现焊前预热可以显著降低焊接接头的残余应力。采用数值模拟计算了不同预热温度下温度场和应力场的变化情况,获得了不同预热温度条件下热应力的动态变化规律,揭示了预热降低残余应力的内在机理。对比2种预处理工艺焊接接头熔合区和热影响区的显微组织、元素分布和晶粒取向,进一步阐明了预热可以通过促进元素扩散和诱发变体选择降低β→α相变产生的应力集中。

关键词 : 钛合金,  残余应力,  中子衍射,  显微组织,  力学性能    
Abstract:

Welding is an essential means of joining structural components to form a new structure. Welding residual stress mainly results from materials expanding or contracting due to temperature variations, which can reduce the life of titanium alloys. Therefore, to reduce undesired residual stress, the welding process and microstructure of the materials involved should be optimized. Titanium alloys play a crucial role in marine and aviation fields due to their excellent corrosion resistance and high specific strength. This work investigates the influence mechanism of the prewelding pretreatment process on the structure, mechanical properties, and residual stress of the electron beam welding joint of a titanium alloy thick plate. The macrostructure and microstructure of titanium alloy welding joints prepared using different pretreatment processes are characterized. Results showed that preheating before welding substantially widens the fusion zone (FZ) and heat-affected zone (HAZ) of the welding joint, coarsening α lamellae in both zones. Thus, the hardness of the FZ and HAZ of the preheated welding joint is reduced to close to that of the base metal. Simultaneously, the strength and toughness of the welding joint is considerably improved such that it is similar to the base metal. The neutron diffraction, deep-hole drilling, and Rostenthal-Norton contour methods are used to measure the residual stress of the electron beam welding joint. The neutron diffraction method exhibits high detection accuracy and can achieve stress monitoring in different zones of the weld seam. Deep-hole drilling is a mechanical strain relief technique for measuring transverse and longitudinal residual stress through component thickness. The Rostenthal-Norton contour method can obtain a three-dimensional stress on the welding joint. A combination of these three measurement techniques can complement and be used to verify each other, providing reasonable data for the residual stress evaluation. The detection results of unpreheated welding joints are compared and analyzed, and the residual stress distribution in the FZ and HAZ zones along different directions is obtained. The FZ is subjected to tensile residual stress along all three directions. Alternatively, the HAZ is subjected to compressive stress along the transverse and longitudinal directions and tensile stress along the normal direction. The residual stress at base metal is small. Additionally, the residual stress results obtained by the deep-hole drilling method for the welding joints using two preheating processes are compared. The results showed that preheating before welding can considerably reduce residual stress at the weld. The reason is discussed in depth. Numerical simulation is used to calculate the changes in the temperature and stress fields under different preheating temperatures. The dynamic change rules of thermal stress under different preheating temperatures are obtained. Results showed that increasing the preheating temperature reduces thermal stress and the thermal expansion mismatch in different areas of the welded joint. Moreover, the microstructure, element distribution, and grain orientation of the FZ and HAZ of joints welded using two pretreatment processes are analyzed. Preheating coarsens the α lamellae and promotes the redistribution of alloy elements, thereby reducing the stress concentration between α and β phases. Besides, variant selection of the HAZ is induced by the preheating process. The number and differences in the orientation of α variants are decreased, thereby reducing the stress concentration between variants.

Key words: titanium alloy    residual stress    neutron diffraction    microstructure    mechanical property
收稿日期: 2024-02-28     
ZTFLH:  TG40  
基金资助:国家重点研发计划项目(2021YFC2801801);中国科学院依托重大科技基础设施的建制化科研项目(JZHKYPT-2021-01)
通讯作者: 马英杰,yjma@imr.ac.cn,主要从事结构钛合金研究王延绪,yxwang@imr.ac.cn,主要从事固态相变、变形机理的中子散射研究
Corresponding author: MA Yingjie, professor, Tel: 13840026329, E-mail: yjma@imr.ac.cnWANG Yanxu, professor, Tel: 18525069032, E-mail: yxwang@imr.ac.cn
作者简介: 周 牧,女,2000年生,硕士生
王 倩,女,1992年生,博士(共同第一作者)
图1  不同残余应力检测方法的取样示意图及中子衍射(ND)法样品放置示意图
图2  钛合金板材原始组织形貌的OM像
图3  未预热和预热钛合金焊接接头的OM像
Welding conditionFZHAZNear- FZMid-HAZNear-BM
Unpreheated5.064.411.921.431.06
Preheated8.048.724.023.021.68
表1  未预热和预热钛合金焊接接头不同区域的宽度 (mm)
图4  未预热和预热钛合金焊接接头熔合区(FZ)和母材(BM)的SEM像
图5  未预热和预热钛合金焊接接头距熔合线不同距离处热影响区(HAZ)的SEM像
图6  未预热和预热焊接接头Vickers硬度分布
Welding condition

Rp0.2

MPa

Rm

MPa

A

%

I / J
FZ-NDNFZ-RDHAZ-NDNHAZ-RD
Unpreheated937.3998.39.79.711.214.714.0
Preheated902.3997.710.827.028.028.031.0
表2  未预热和预热焊接接头力学性能
图7  ND法无应力样品不同探测器(D1、D2) 4 h的检测曲线和(101) α 晶面间距拟合结果
图8  不同方法获得的焊接残余应力检测结果对比
图9  未预热焊接接头不同位置ND法残余应力检测结果
图10  不同预热温度下焊接过程中焊接接头中心位置的平均温度和残余应力
图11  未预热和预热焊接接头HAZ的SEM像及EPMA像
图12  未预热和预热焊接接头HAZ的EBSD像
1 Aba-Perea P E, Pirling T, Preuss M. In-situ residual stress analysis during annealing treatments using neutron diffraction in combination with a novel furnace design [J]. Mater. Des., 2016, 110: 925
2 Lim S H, Zhang Z, Seng D H L, et al. In-situ warm shot peening on Ti-6Al-4V alloy: Effects of temperature on fatigue life, residual stress, microstructure and mechanical properties [J]. J. Alloys Compd., 2021, 882: 160701
3 Sun G A, Chen B. The technology and application of residual stress analysis by neutron diffraction [J]. Nucl. Tech., 2007, 30(4):286
3 孙光爱, 陈 波. 中子衍射残余应力分析技术及其应用 [J]. 核技术, 2007, 30(4): 286
4 Woo W, Em V, Hubbard C R, et al. Residual stress determination in a dissimilar weld overlay pipe by neutron diffraction [J]. Mater. Sci. Eng., 2011, A528: 8021
5 Ren Y, Paradowska A, Wang B, et al. Residual stress state of X65 pipeline girth welds before and after local and furnace post weld heat treatment [J]. J. Pressure Vessel Technol., 2017, 139: 041401
6 Liu T, Bunn J R, Fancher C M, et al. Neutron diffraction analysis of residual strain in high-pressure die cast A383 engine blocks [J]. J. Mater. Eng. Perform., 2020, 29: 5428
7 Burca G, James J A, Kockelmann W, et al. A new bridge technique for neutron tomography and diffraction measurements [J]. Nucl. Instrum. Methods Phys. Res., 2011, 651A: 229
8 Li S L, Li Y, Wang Y K, et al. Multiscale residual stress evaluation of engineering materials/components based on neutron and synchrotron radiation technology [J]. Acta Metall. Sin., 2023, 59: 1001
doi: 10.11900/0412.1961.2023.00157
8 李时磊, 李 阳, 王友康 等. 基于中子与同步辐射技术的工程材料/部件多尺度残余应力评价 [J]. 金属学报, 2023, 59: 1001
doi: 10.11900/0412.1961.2023.00157
9 Zhang Z W, Feng Y F, Tan Q, et al. Residual stress distribution in Ni-based superalloy turbine discs during fabrication evaluated by neutron/X-ray diffraction measurement and thermomechanical simulation [J]. Mater. Des., 2019, 166: 107603
10 Song S P, Paradowska A M, Dong P S. Investigation of residual stresses distribution in titanium weldments [J]. Mater. Sci. Forum, 2014, 777: 171
11 Lin Y C, Lee K H. Effect of preheating on the residual stress in type 304 stainless steel weldment [J]. J. Mater. Process. Technol., 1997, 63: 797
12 Asadi P, Alimohammadi S, Kohantorabi O, et al. Effects of material type, preheating and weld pass number on residual stress of welded steel pipes by multi-pass TIG welding (C-Mn, SUS304, SUS316) [J]. Therm. Sci. Eng. Prog., 2020, 16: 100462
13 Malý M, Höller C, Skalon M, et al. Effect of process parameters and high-temperature preheating on residual stress and relative density of Ti6Al4V processed by selective laser melting [J]. Materials, 2019, 12: 930
14 Chen B, Skouras A, Wang Y Q, et al. In situ neutron diffraction measurement of residual stress relaxation in a welded steel pipe during heat treatment [J]. Mater. Sci. Eng., 2014, A590: 374
15 Yan G X, Crivoi A, Sun Y J, et al. An Arrhenius equation-based model to predict the residual stress relief of post weld heat treatment of Ti-6Al-4V plate [J]. J. Manuf. Process., 2018, 32: 763
16 Lombardi A, Sediako D, Machin A, et al. Effect of solution heat treatment on residual stress in Al alloy engine blocks using neutron diffraction [J]. Mater. Sci. Eng., 2017, A697: 238
17 Wang B, Zhou L, Cao Y S, et al. Analysis of residual stress relief for Ti62A alloy welded joints by post weld heat treatment considering creep effect [J]. J. Mater. Res. Technol., 2023, 24: 7462
18 Wei H. Effect of texture on properties and residual stress in Cu-Ni-Si alloys and its mechanism [D]. Beijing: University of Science and Technology Beijing, 2021
18 韦 贺. 铜镍硅系合金中织构对性能和残余应力的影响及作用机制 [D]. 北京: 北京科技大学, 2021
19 Zhu W X. Study on residual stress reduction process of GH4169 alloy rings [D]. Guizhou: Guizhou University, 2021
19 朱文祥. GH4169合金环件残余应力消减工艺研究 [D]. 贵州: 贵州大学, 2021
20 Zhang K Y, Dong W C, Zhao D, et al. Effect of solid-state phase transformation on stress and distortion for Fe-Co-Ni ultra-high strength steel components during welding and vacuum gas quenching processes [J]. Acta Metall. Sin., 2023, 59: 1633
20 张开元, 董文超, 赵 栋 等. 固态相变对Fe-Co-Ni超高强度钢长臂梁构件焊接-淬火过程应力和变形的影响 [J]. 金属学报, 2023, 59: 1633
doi: 10.11900/0412.1961.2022.00177
21 Etesami S A, Fotovvati B, Asadi E. Heat treatment of Ti-6Al-4V alloy manufactured by laser-based powder-bed fusion: Process, microstructures, and mechanical properties correlations [J]. J. Alloys Compd., 2022, 895: 162618
22 Lou Y H, Lin G X, Liu Y P, et al. Effect of post-weld heat treatment on microstructure and mechanical properties of electron beam welded TC4 joints [J]. Hot Work. Technol., 2013, 42(19): 179
22 娄宇航, 蔺广学, 刘俞平 等. TC4真空电子束焊后热处理对接头组织性能的影响 [J]. 热加工工艺, 2013, 42(19): 179
23 Brinson H F, Brinson L C. Stress and strain analysis and measurement [A]. Polymer Engineering Science and Viscoelasticity: An Introduction [M]. New York: Springer, 2015: 15
24 Chen J, Jiang Y L, Chen H N. Three-dimensional residual stress determination in Q345 weldment before and after PWHT by deep-hole drilling method [J]. Weld. J., 2022, (12): 25
24 陈 静, 姜云禄, 陈怀宁. 深孔法测试Q345焊接试板热处理前后三维残余应力的可行性 [J]. 焊接, 2022, (12): 25
25 Pederson R, Niklasson F, Skystedt F, et al. Microstructure and mechanical properties of friction- and electron-beam welded Ti-6Al-4V and Ti-6Al-2Sn-4Zr-6Mo [J]. Mater. Sci. Eng., 2012, A552: 555
26 Zhang S L, Ma Y J, Huang S S, et al. Temperature-gradient induced microstructure evolution in heat-affected zone of electron beam welded Ti-6Al-4V titanium alloy [J]. J. Mater. Sci. Technol., 2019, 35: 1681
doi: 10.1016/j.jmst.2019.04.004
27 Attallah M M, Preuss M, Boonchareon C, et al. Microstructural and residual stress development due to inertia friction welding in Ti-6246 [J]. Metall. Mater. Trans., 2012, 43A: 3149
28 Hall E O. The deformation and ageing of mild steel: III Discussion of results [J]. Proc. Phys. Soc., 1951, 64B: 747
29 Owen C, Jeffs S, Perkins K, et al. The evolution of Ti-6Al-4V following extreme thermo-mechanical processing [A]. Proceedings of the 13th World Conference on Titanium [C]. Hoboken: John Wiley & Sons, Inc., 2016: 456
30 Rae W, Lomas Z, Jackson M, et al. Measurements of residual stress and microstructural evolution in electron beam welded Ti-6Al-4V using multiple techniques [J]. Mater. Charact., 2017, 132: 10
31 Xu W W, Shang S L, Zhou B C, et al. A first-principles study of the diffusion coefficients of alloying elements in dilute α-Ti alloys [J]. Phys. Chem. Chem. Phys., 2016, 18: 16870
doi: 10.1039/c6cp01899h pmid: 27282515
[1] 朱桂杰, 王思清, 查敏, 李眉娟, 孙凯, 陈东风. 稀土元素Ce对挤压态Mg-0.3Al-0.2Ca-0.5Mn合金板材体织构及力学各向异性的影响[J]. 金属学报, 2024, 60(8): 1079-1090.
[2] 谷黎明, 冯效铭, 于朝, 张峻凡, 刘振宇, 何伦华, 卢怀乐, 李小虎, 王晨, 张晓东, 肖伯律, 马宗义. 深冷循环对SiC/Al复合材料宏微观残余应力的影响[J]. 金属学报, 2024, 60(8): 1031-1042.
[3] 任卫军, 安萌, 高飞, 罗小华, 李昺, 张志东, 王进威. 三方Cr5Te8 的磁结构和反常热膨胀[J]. 金属学报, 2024, 60(8): 1150-1154.
[4] 李彪, 张龙, 颜廷毅, 付华萌, 袁旭东, 文明月, 张宏伟, 李宏, 张海峰. 热处理工艺和W丝特性对W丝增强锆基非晶复合材料残余应力的影响[J]. 金属学报, 2024, 60(8): 1055-1063.
[5] 王浩宇, 吕熙睿, 陈琦, 熊瑛, 罗志新, 张洁, 王京阳. 高熵稀土单硅酸盐环境障涂层局域结构的原子对分布函数解析[J]. 金属学报, 2024, 60(8): 1130-1140.
[6] 林皓, 李建, 杨钊龙, 钟圣怡. 中子衍射应力分析技术及其应用进展[J]. 金属学报, 2024, 60(8): 1017-1030.
[7] 陈诚, 杨光昱, 金梦辉, 王强, 汤鑫, 程会民, 介万奇. 铸型正反转搅动对精密铸造K4169合金凝固组织和室温力学性能的影响[J]. 金属学报, 2024, 60(7): 926-936.
[8] 孟玉佳, 席通, 杨春光, 赵金龙, 张新蕊, 于英杰, 杨柯. Ga添加对304L不锈钢力学性能和抗菌性能的影响[J]. 金属学报, 2024, 60(7): 890-900.
[9] 谢丽文, 张立龙, 刘艳艳, 张明阳, 王绍钢, 焦大, 刘增乾, 张哲峰. 不锈钢纤维增强镁基仿生复合材料制备与力学性能[J]. 金属学报, 2024, 60(6): 760-769.
[10] 王峰, 白盛巍, 王志, 杜旭东, 周乐, 毛萍莉, 魏子淇, 李瑾伟. Mg-Zn系合金热裂行为的研究进展[J]. 金属学报, 2024, 60(6): 743-759.
[11] 许仁杰, 屠鑫, 胡斌, 罗海文. Cu-V双合金化3Mn钢的组织和力学性能[J]. 金属学报, 2024, 60(6): 817-825.
[12] 熊毅, 栾泽伟, 马云飞, 厉勇, 查小琴. 超音速微粒轰击诱导表面纳米化对300M钢腐蚀疲劳行为的影响[J]. 金属学报, 2024, 60(5): 627-638.
[13] 李天瑞, 许瑜倩, 吴文平, 甘文萱, 杨永, 刘国怀, 王昭东. V和B元素对Ti-44Al-5Nb-1Mo合金显微组织及热变形机制的影响[J]. 金属学报, 2024, 60(5): 650-660.
[14] 曾立, 王桂兰, 张海鸥, 翟文正, 张勇, 张明波. 电弧微铸锻复合增材制造GH4169D高温合金的显微组织与力学性能[J]. 金属学报, 2024, 60(5): 681-690.