Effect of Annealing Heat Treatment on the Macroscopic and Microscopic Deformation Behavior of Additively Manufactured AlSi10Mg Alloy
ZHANG Xingxing1(), LUTZ Andreas2, GAN Weimin3, MAAWAD Emad3, KRIELE Armin4
1 Multi-disciplinary Research Division, Institute of High Energy Physics, Chinese Academy of Sciences, Beijing 100049, China 2 Mercedes Benz AG, Research and Development Department, Leibnizstr. 2, 71032 Böblingen, Germany 3 Institute of Materials Physics, Helmholtz-Zentrum Hereon, Max-Planck-Str. 1, 21502 Geesthacht, Germany 4 German Engineering Materials Science Centre (GEMS) at Heinz Maier-Leibnitz Zentrum (MLZ), Helmholtz-Zentrum Hereon, 85748 Garching, Germany
Cite this article:
ZHANG Xingxing, LUTZ Andreas, GAN Weimin, MAAWAD Emad, KRIELE Armin. Effect of Annealing Heat Treatment on the Macroscopic and Microscopic Deformation Behavior of Additively Manufactured AlSi10Mg Alloy. Acta Metall Sin, 2024, 60(8): 1091-1099.
The additively manufactured AlSi10Mg alloy demonstrates considerable residual stresses, adversely affecting the dimensional accuracy, operational safety, and corrosion resistance of the parts. In practical applications, stress relief annealing is necessary to eliminate residual stresses in residual stress-sensitive applications. However, the current understanding of the mechanical properties of the additively manufactured AlSi10Mg alloy after annealing is still limited to the macroscopic level. To further investigate the micromechanical behavior and intrinsic mechanisms of the alloy, this study employed synchrotron X-ray diffraction technology to conduct in situ deformation analysis. This study thoroughly examined the lattice strain and stress evolutions of the Al and Si phases and clarified the individual contribution of each phase to the strain hardening rate of the alloy. In addition, this study quantitatively assessed the evolution of dislocation density and elucidated the influences of annealing heat treatment on the load transfer and dislocation behavior of the additively manufactured AlSi10Mg alloy.
Fig.1 Sample dimensions for the in situ deformation experiment (unit: mm) (a) as-printed sample (b) stress-relieved annealed sample
Fig.2 Macroscopic behaviors of as-built and annealed samples (a) engineering stress-strain curves (b) hardening coefficient curves (c) determination of uniform true strain
Fig.3 SEM images of microstructures of as-built (a-c) and annealed (d-f) samples (a, d) microstructures at low magnification (b, e) microstructures within the melt-pool (c, f) microstructures on the melt-pool boundary
Fig.4 Evolutions of lattice strains of as-built (a, c) and annealed (b, d) samples (LD—loading direction, TD—transverse direction) (a, b) Al matrix (c, d) Si phase
Sample
Direction
Al{111}
Al{200}
Al{220}
Al{311}
Si{111}
Si{220}
Si{311}
Si{422}
As-built
LD
16.86
15.58
20.11
20.57
182.73
2467.52
209.37
308.45
TD
49.80
24.88
15.74
26.65
141.62
1574.93
295.66
281.45
Annealed
LD
29.40
30.40
14.51
26.19
83.85
2019.93
105.50
97.65
TD
51.04
34.36
14.37
34.36
95.04
568.67
76.91
95.85
Table 1 Maximum lattice strain errors during whole deformation process
Fig.5 Evolutions of phase stresses of as-built (a, c) and annealed (b, d) samples (a, b) Al matrix (c, d) Si phase
Fig.6 Dislocation density evolutions of Al matrix of as-built and annealed samples
Fig.7 Contributions of Al and Si phases to the strain hardening rate of the alloys (The data of alloys in Fig.2b was plotted here again for comparison) (a) as-built sample (b) annealed sample
1
Aboulkhair N T, Simonelli M, Parry L, et al. 3D printing of aluminium alloys: Additive manufacturing of aluminium alloys using selective laser melting [J]. Prog. Mater Sci., 2019, 106: 100578
2
Martin J H, Yahata B D, Hundley J M, et al. 3D printing of high-strength aluminium alloys [J]. Nature, 2017, 549: 365
3
Fiocchi J, Tuissi A, Biffi C A. Heat treatment of aluminium alloys produced by laser powder bed fusion: A review [J]. Mater. Des., 2021, 204: 109651
4
Zhao L, Macías J G S, Dolimont A, et al. Comparison of residual stresses obtained by the crack compliance method for parts produced by different metal additive manufacturing techniques and after friction stir processing [J]. Addit. Manuf., 2020, 36: 101499
5
Schröder J, Evans A, Mishurova T, et al. Diffraction-based residual stress characterization in laser additive manufacturing of metals [J]. Metals, 2021, 11: 1830
6
Fang Z C, Wu Z L, Huang C G, et al. Review on residual stress in selective laser melting additive manufacturing of alloy parts [J]. Opt. Laser Technol., 2020, 129: 106283
7
Laleh M, Sadeghi E, Revilla R I, et al. Heat treatment for metal additive manufacturing [J]. Prog. Mater Sci., 2023, 133: 101051
8
Huang N, Luo Q X, Bartles D L, et al. Effect of heat treatment on microstructure and mechanical properties of AlSi10Mg fabricated using laser powder bed fusion [J]. Mater. Sci. Eng., 2024, A895: 146228
9
Takata N, Kodaira H, Sekizawa K, et al. Change in microstructure of selectively laser melted AlSi10Mg alloy with heat treatments [J]. Mater. Sci. Eng., 2017, A704: 218
10
Chen S Q, Tan Q Y, Gao W Q, et al. Effect of heat treatment on the anisotropy in mechanical properties of selective laser melted AlSi10Mg [J]. Mater. Sci. Eng., 2022, A858: 144130
11
Zhang C C, Zhu H H, Liao H L, et al. Effect of heat treatments on fatigue property of selective laser melting AlSi10Mg [J]. Int. J. Fatigue, 2018, 116: 513
12
Tridello A, Fiocchi J, Biffi C A, et al. Influence of the annealing and defects on the VHCF behavior of an SLM AlSi10Mg alloy [J]. Fatigue Fract. Eng. Mater. Struct., 2019, 42: 2794
13
Xie Q G, Lian J H, Sidor J J, et al. Crystallographic orientation and spatially resolved damage in a dispersion-hardened Al alloy [J]. Acta Mater., 2020, 193: 138
14
Zhang X X, Lutz A, Andrä H, et al. Evolution of microscopic strains, stresses, and dislocation density during in-situ tensile loading of additively manufactured AlSi10Mg alloy [J]. Int. J. Plast., 2021, 139: 102946
15
Takata N, Liu M L, Hirata M, et al. Microstructural origins of high strength of Al-Si alloy manufactured by laser powder bed fusion: In-situ synchrotron radiation X-ray diffraction approach [J]. J. Mater. Sci. Technol., 2024, 178: 80
16
Li C, Zhang W X, Yang H O, et al. Microstructural origin of high strength and high strain hardening capability of a laser powder bed fused AlSi10Mg alloy [J]. J. Mater. Sci. Technol., 2024, 197: 194
17
Hong Y Y, Gao J, Liu X Q, et al. Investigation of the high-temperature fatigue mechanism related to altered local short-range order in AL6XN austenitic stainless steel [J]. Mater. Des., 2023, 236: 112504
18
Masumura T, Inami K, Matsuda K, et al. Quantitative evaluation of dislocation density in as-quenched martensite with tetragonality by X-ray line profile analysis in a medium-carbon steel [J]. Acta Mater., 2022, 234: 118052
19
Ribárik G, Jóni B, Ungár T. Global optimum of microstructure parameters in the CMWP line-profile-analysis method by combining Marquardt-Levenberg and Monte-Carlo procedures [J]. J. Mater. Sci. Technol., 2019, 35: 1508
doi: 10.1016/j.jmst.2019.01.014
20
Zhang X X, Bauer P P, Lutz A, et al. Microplasticity and macroplasticity behavior of additively manufactured Al-Mg-Sc-Zr alloys: In-situ experiment and modeling [J]. Int. J. Plast., 2023, 166: 103659
21
Zhang X X, Lutz A, Andrä H, et al. An additively manufactured and direct-aged AlSi3.5Mg2.5 alloy with superior strength and ductility: Micromechanical mechanisms [J]. Int. J. Plast., 2021, 146: 103083
22
Li Y, Yu J Y, Li S L, et al. The influence of post-aging treatment on the microstructure and micromechanical behaviors of additively manufactured maraging steel investigated by in situ high-energy X-ray diffraction [J]. J. Mater. Sci. Technol., 2024, 200: 1
23
Zhang X X, Knoop D, Andrä H, et al. Multiscale constitutive modeling of additively manufactured Al-Si-Mg alloys based on measured phase stresses and dislocation density [J]. Int. J. Plast., 2021, 140: 102972
24
Harjo S, Tsuchida N, Abe J, et al. Martensite phase stress and the strengthening mechanism in TRIP steel by neutron diffraction [J]. Sci. Rep., 2017, 7: 15149
doi: 10.1038/s41598-017-15252-5
pmid: 29123143
25
Zhang X X, Lutz A, Andrä H, et al. Strain hardening behavior of additively manufactured and annealed AlSi3.5Mg2.5 alloy [J]. J. Alloys Compd., 2022, 898: 162890
26
Santos Macías J G, Douillard T, Zhao L, et al. Influence on microstructure, strength and ductility of build platform temperature during laser powder bed fusion of AlSi10Mg [J]. Acta Mater., 2020, 201: 231
27
Dan C Y, Cui Y C, Wu Y, et al. Achieving ultrahigh fatigue resistance in AlSi10Mg alloy by additive manufacturing [J]. Nat. Mater., 2023, 22: 1182
doi: 10.1038/s41563-023-01651-9
pmid: 37592031