Please wait a minute...
金属学报  2019, Vol. 55 Issue (1): 109-125    DOI: 10.11900/0412.1961.2018.00307
  本期目录 | 过刊浏览 |
金属基复合材料高通量制备及表征技术研究进展
张学习1, 郑忠1, 高莹2, 耿林1()
1 哈尔滨工业大学材料科学与工程学院 哈尔滨 150001
2 北京空间飞行器总体设计部 北京 100086
Progress in High Throughput Fabrication and Characterization of Metal Matrix Composites
Xuexi ZHANG1, Zhong ZHENG1, Ying GAO2, Lin GENG1()
1 School of Materials Science and Engineering, Harbin Institute of Technology, Harbin 150001, China
2 Institute of Spacecraft System Engineering, Beijing 100086, China
引用本文:

张学习, 郑忠, 高莹, 耿林. 金属基复合材料高通量制备及表征技术研究进展[J]. 金属学报, 2019, 55(1): 109-125.
Xuexi ZHANG, Zhong ZHENG, Ying GAO, Lin GENG. Progress in High Throughput Fabrication and Characterization of Metal Matrix Composites[J]. Acta Metall Sin, 2019, 55(1): 109-125.

全文: PDF(7658 KB)   HTML
摘要: 

“材料基因工程”计划是以大数据作为支撑,采用高通量设计、制备和表征技术,促使材料研究从传统的试错模式转向低成本、快速响应的新模式,从而加快新材料的研发速度,实现研发成本和周期“双减半”的目标。金属基复合材料由于组分复杂、制备过程为热力学非平衡状态,带来一些新的问题需要解决,包括:(1) 高通量制备方法方面,针对合金块体样品开发的喷印合成法、多元结扩散法等基于热力学平衡理论的高通量制备技术无法直接用于金属基复合材料构件块体坯料的制造;(2) 高通量表征技术方面,缺乏针对金属基复合材料单一样品成分、形貌、组织、结构和性能的多维、多场、多尺度同步采集技术,以及针对阵列样品成分、形貌、组织与结构的快速表征技术。鉴于上述问题,本文综述了金属基复合材料高通量制备及表征技术发展现状及已取得的进展,特别是在增强体呈梯度分布的金属基复合材料制备技术与高通量组合表征方法上取得的突破,推动了高通量制备及表征技术在金属基复合材料领域的应用。最后指出了金属基复合材料高通量计算、制备方法和表征技术方面存在的瓶颈问题,并对高通量制备与表征技术的发展进行了展望。

关键词 : 金属基复合材料,  高通量制备,  高通量表征,  梯度复合材料,  研究现状    
Abstract:

The "material genetic engineering" plan, based on the large data, is to investigate the high throughput design, fabrication and characterization techniques with the aim to shift the material research from traditional mode to high throughput mode with low cost and fast response speed, and to accelerate the research and development of new materials and achieve the goal of "double reduction halves". As the metal matrix composites (MMCs) exhibit multi-components and a thermodynamically non-equilibrium state during fabrication, some key issues occur and need to be addressed including: (1) for high throughput fabrication, currently developed high throughput technologies based on thermodynamically equilibrium conditions, such as spray printing and multi-node diffusion methods, are not applicable for MMCs; (2) for high throughput characterization, there is a lack of multi- dimensional, field and scale acquisition technique for the composition, morphology, microstructure and property of MMCs. In order to solve these problems, the progress on the research and development of high throughput fabrication and characterization techniques of MMCs was reviewed, especially, in the field of gradient reinforced MMCs and their high throughput combination characterization methods, which may promote the application of high throughput fabrication and characterization techniques in MMCs. Finally, the bottlenecks and prospects in the high throughput fabrication and characterization of MM Cs are proposed.

Key words: metal matrix composites (MMCs)    high throughput fabrication    high throughput characterization    gradient metal matrix composites (GMMCs)    research status
收稿日期: 2018-07-03     
ZTFLH:  TG457  
基金资助:国家重点研发计划项目No.2017YFB0703103
作者简介:

作者简介 张学习,男,1975年生,教授,博士

图1  材料的传统研发模式与高通量研发模式对比
Technique Application area Advantage Ref.
Co-deposition method High throughput preparation of multi-component alloys Precise control of composition and gradient distribution [4,33]
Discrete template coating Doping of epitaxial films with transition metals and synthesis of sulfuric semiconductor materials Uniform, controllable and wide span composition and unlimited number of components [4,5]
Continuous template coating Preparation of dielectric materials and study of multi-alloy phase diagrams Controllable component distribution and continuous linear distribution states [35,36]
Spray printing Preparing combined ceramic specimens Repeated delivery of multiple components in a fast and precise way [9~11]
Microfluidic structure method Preparation and characterization of trace amount of catalysts Fast response to stress, helpful in conducting efficient characterization [37~39]
Multiple diffusion nodes Drawing three element phase diagrams and quickly screening materials Gaining alloys with gradient composition changes [6~8]
Microelectromechani-cal structure Studying mechanical properties and transformation enthalpies of alloys Quickly examine many samples, high compatibility with high-throughput experiments [16,17,21]
Chemical bath deposition Preparation of array film materials High efficiency for films, suitable for multi-component systems [40]
Magnetron sputtering Preparing film samples with various elements and contents High efficiency in preparing multi-component films [14]
Multi-flow pulse laser deposition High-throughput synthesis of monolayer and multilayer thin films Composite films have uniform composition and high performance [41]
Direct atomization of oligomers High throughput preparation of nano-scale hybrid membranes Low defect density in nano hybrid membranes and high fabrication efficiency [42]
Cooling rate controlling Studying correlation between cooling rate and properties of polycrystalline nickel based alloys High efficiently characterizing the correlation between microstructures and properties [43]
High throughput sintering diffusion Synthesis of magnetic materials Study of the new phases and equilibrium phases in alloys [44]
Linear friction welding Fabrication of alloys with gradient element distribution state Establishing the relationship among element content, microstructure and properties [45]
Focused ion beam machining Any area of interest can be collected in many kinds of materials Preparing micron- or nano-samples for direct analysis of microstructure and properties [46]
Laser additive manufacturing Preparing alloys, composites and micron- or nano-structured materials High precision in dimensions and wide range of application [47~50]
表1  金属材料高通量制备方法、原理、应用及优点分析[4~11,14,16,17,21,33,35~50]
Method Application area Ref.
Selective laser cladding Creation of gradient component distribution in Si/Al composites by tailoring vaporization of Al under laser and unidirectional solidification under external magnetic fields [12,13]
Centrifugal casting Ni powders of various sizes were distributed in Al2O3 under centrifugal process of the mixed slurry [51]
Uniaxial hot pressing Creation of gradient distribution of density, hardness, porosity and pore size in Al2O3/C composites by inhomogeneous temperature distribution during hot pressing [52]
Laminating Preparing laminated Al composite materials with 2%, 4% and 6% (volume fraction) SiC particles via hot pressing [53]
Positioning impregnation Preparing Ti3SiC2/SiC composites with graded components by hot pressing and impregnation at high temperature [54]
表2  金属基复合材料高通量制备方法和应用领域[12,13,51~54]
图2  变形前后SiCp/Al复合材料界面微柱SEM像[57]
图3  静电自组装制备石墨烯呈梯度分布的石墨烯-Al粉混合粉
图4  多道次冷拉拔制备石墨烯/Al复合材料丝材过程和组织[59]
图5  层状金属基复合材料通过热挤压和拉拔获得复合材料纤维的示意图
图6  TiCp/Ti6Al4V复合材料网状结构SEM像[60]
图7  基于粉末冶金的网状钛基复合材料高通量制备技术
图8  基于无压浸渗的铝基复合材料高通量制备技术
图9  采用聚焦离子束加工金属基复合材料微小样品阵列
Technique Applicable area Reference
X-ray diffraction (XRD) Phase information [65]
Atomic force microscopy (AFM) Surface roughness and three-dimensional image [66]
Scanning probe Characterizing electro-catalysts and electrodes with gradient component distribution [67~69]
X-ray photoelectron spectroscopy Quantitative analysis of surface compositions and functional groups [70,71]
Secondary ion mass spectroscopy
Qualitative analysis of the surface compositions (acting as supplement of X-ray photoelectron spectrum using molecular ion segment spectrum) [70,71]
In situ XRD The evolution of the crystal structure in the stress field, temperature field and combination of these fields [72,73]
X-ray absorption near edge spectrum High resolution characterization of the large volume 2D and 3D morphologies (tens of nanometers) and chemical compositions [74,75]
Neutron diffraction technique Three dimensional spatial distribution of texture evolution, microstructure and residual stress in bulk materials [76~78]
Decalescent microwave probe microscopy Characterization of electrical (superconductivity, conductivity, dielectric constant etc.) and magnetic (magnetic susceptibility and spin resonance etc.) properties [79,80]
Nano scanning calorimetry Characterization of the thermodynamic parameters such as enthalpy, heat capacity and phase transition temperature [21~23]
X-ray fluorescence technique Chemical composition, elemental analysis and identification [65]
Near edge X-ray absorption spectroscopy Characterization of the element valence state [65]
Ultraviolet-visible spectroscopy The absorbance characteristics and molecular conjugation analysis [31]
Infrared emission imaging Screening organic and inorganic materials and hydrogen storage metal materials [81]
Mass spectrometry Mass ratio analysis and compound/molecular identification [82]
Gas chromatography Separation and identification of the complex [83]
Resonance enhanced multiphoton ionization Study of the spectrum and molecular rotation information of atoms and small molecules [31]
In situ X-ray absorption spectroscopy Characterization of the chemical evolution [74,84]
In situ X-ray binding mass spectrometry Characterization of the thermal stability [74]
Cantilever beam array technology Thermomechanical behavior analysis of thin films with wide component gradient [85]
Nuclear magnetic resonance spectrum Analyzing small stray magnetic field and relaxation phenomena of small magnets [86,87]
Photoacoustic technology Identification and characterization of parallel catalytic products [88]
表3  金属基复合材料显微组织表征技术及其应用领域[21~23,31,65~88]
Technique Application area Reference
Ion beam analysis Automatic detection for abundant samples; promising for high throughput detection [89]
High throughput transmission technology Characterization of composition phases, development of new materials and construction of phase diagrams [25]
In situ transmission electron microscopy (TEM) Simultaneous in-situ imaging and electrical measurement, and observation of grain growth process induced by electric current [90]
Differential aperture XRD technique Low X-ray energy, sub-micron size of the spot, fairly high spatial resolution, and useful for analyzing deformation microstructures [91]
Three dimensional XRD technique High spatial and angular resolutions, suitable for studying recrystallization growth process [24]
Automatic scanning nano-indentation technology Mechanical properties of small volume materials, including strength and modulus [18,85,92~94]
Optical microscopy combined with differential interference imaging Three-dimensional surface topography and height information at re-melting lines [26~28]
Laser induced fluorescence imaging technology High throughput in-situ screening with micron scale spatial resolution and millisecond time resolution [95]
Scanning X-ray fluorescence microscopy Characterization of the element composition and crystal structure [96]
High throughput screening sensor A new high throughput characterization method for a variety of elements [97]
In-situ tensile combined with digital image correlation (DIC) Calculation of the local strain distribution using different strain images, with high spatial resolution and the stretching rate [29]
Scanning electron microscopy (SEM) combined with DIC Precise calculation of image gradients, strain and deformation fields [30]
Femtosecond pulse laser technology Imaging of the time domain thermal reflection for phase formation, with spatial resolution of 1 μm and test rate of 10000 pointsh-1 [15]
Micromechanical testing technology High throughput mechanical properties tests, potential for automatic micro area tests [16~20]
In-situ statistical distribution analysis technique High throughput screening and validation of material design, modification and optimization [98~101]
Multi-dimensional and multi-scale high throughput characterization Three-dimensional crystallographic orientation and reconstruction; material structures; three dimensional X-ray diffraction etc. [102]
Microwave microscopy combined with AFM High spatial resolution characterization of the dielectric/ferroelectric materials [103]
Micro area electrochemical measurement technology High positioning accuracy (resolution 50 nm) and automatic programming tests for high density composite material samples [33]
表4  金属基复合材料性能高通量表征技术和应用领域[15~20,24~30,33,85,89~103]
图10  层状复合材料组织、变形以及力学性能同步表征技术示意图[29]
图11  改进的X射线衍射仪及其应用[104]
图12  基于同步辐射的电极复合材料原位表征技术[105]
图13  时域探测激光束偏转(TD-PBD)方法的原理及其精度分析[106]
图14  基于SEM的金属基复合材料高通量表征平台
图15  基于X射线同步辐射的金属基复合材料高通量表征平台
图16  阵列样品快速表征技术示意图
[1] Huang L J, Geng L, Peng H X.Microstructurally inhomogeneous composites: Is a homogeneous reinforcement distribution optimal?[J]. Prog. Mater. Sci., 2015, 71: 93
[2] Hattrick-Simpers J, Wen C, Lauterbach J.The materials super highway: Integrating high-throughput experimentation into mapping the catalysis materials genome[J]. Catal. Lett., 2015, 145: 290
[3] Zhao J C.A perspective on the materials genome initiative[J]. Chin. J. Nat., 2014, 36: 89(赵继成. 材料基因组计划简介[J]. 自然杂志, 2014, 36: 89)
[4] Mao S S.High throughput growth and characterization of thin film materials[J]. J. Cryst. Growth, 2013, 379: 123
[5] Jin Z W, Murakami M, Fukumura T, et al. Combinatorial laser MBE synthesis of 3d ion doped epitaxial ZnO thin films [J]. J. Cryst. Growth, 2000, 214-215: 55
[6] Zhao J C, Jackson M R, Peluso L A, et al.A diffusion-multiple approach for mapping phase diagrams, hardness, and elastic modulus[J]. JOM, 2002, 54(7): 42
[7] Zhao J C.High-throughput experimental tools for the Materials Genome Initiative[J]. Chin. Sci. Bull., 2014, 58: 3647(赵继成. 材料基因组计划中的高通量实验方法[J]. 科学通报, 2013, 58: 3647)
[8] Wang X, Zhu L L, Fang J, et al.Applications of "Materials Genome Engineering" based methods in nickel-based superalloys[J]. Sci. Technol. Rev., 2015, 33(10): 79(王薪, 朱礼龙, 方姣等. 基于“材料基因组工程”的3种方法在镍基高温合金中的应用[J]. 科技导报, 2015, 33(10): 79)
[9] Wang J S, Yoo Y, Gao C, et al.Identification of a blue photoluminescent composite material from a combinatorial library[J]. Science, 1998, 279: 1712
[10] Chen L, Bao J, Gao C, et al.Combinatorial synthesis of insoluble oxide library from ultrafine/nano particle suspension using a drop-on-demand inkjet delivery system[J]. J. Comb. Chem., 2004, 6: 699
[11] Liu X N, Shen Y, Yang R T, et al.Inkjet printing assisted synthesis of multicomponent mesoporous metal oxides for ultrafast catalyst exploration[J]. Nano Lett., 2012, 12: 5733
[12] Kang N, Coddet P, Wang J, et al.A novel approach to in-situ produce functionally graded silicon matrix composite materials by selective laser melting[J]. Compos. Struct., 2017, 172: 251
[13] Shishkovsky I V, Nazarov P A, Kotoban D V, et al.Comparison of Additive Technologies for Gradient Aerospace Part Fabrication from Nickel-based Superalloys[M]. London: InTech Publ., 2015: 221
[14] Nikoli? V, Wurster S, Savan A, et al.High-throughput study of binary thin film tungsten alloys[J]. Int. J. Refract. Met. Hard Mater., 2017, 69: 40
[15] Huxtable S, Cahill D G, Fauconnier V, et al.Thermal conductivity imaging at micrometre-scale resolution for combinatorial studies of materials[J]. Nat. Mater., 2004, 3: 298
[16] Mccluskey P J, Zhao C W, Kfir O, et al.Precipitation and thermal fatigue in Ni-Ti-Zr shape memory alloy thin films by combinatorial nanocalorimetry[J]. Acta Mater., 2011, 59: 5116
[17] Kim H J, Han J H, Kaiser R, et al.High-throughput analysis of thin-film stresses using arrays of micromachined cantilever beams[J]. Rev. Sci. Instrum., 2008, 79: 045112
[18] Frick C P, Lang T W, Spark K, et al.Stress-induced martensitic transformations and shape memory at nanometer scales[J]. Acta Mater., 2006, 54: 2223
[19] Uchic M D, Dimiduk D M, Florando J N, et al.Sample dimensions influence strength and crystal plasticity[J]. Science, 2004, 305: 986
[20] Vlassak J J, Nix W D.A New bulge test technique for the determination of Young's modulus and Poisson's ratio of thin films[J]. J. Mater. Res., 1992, 7: 3242
[21] Gregoire J M, McCluskey P J, Dale D, et al. Combining combinatorial nanocalorimetry and X-ray diffraction techniques to study the effects of composition and quench rate on Au-Cu-Si metallic glasses[J]. Scr. Mater., 2012, 66: 178
[22] McCluskey P J, Vlassak J J. Combinatorial nanocalorimetry[J]. J. Mater. Res., 2010, 25: 2086
[23] Lee D, Sim G D, Xiao K C, et al.Scanning AC nanocalorimetry study of Zr/B reactive multilayers[J]. J. Appl. Phys., 2013, 114: 214902
[24] Zhang Y B, Fan G H.Three-dimensional X-ray diffraction technique for metals science[J]. Mater. Chin., 2017, 36: 181(张玉彬, 范国华. 三维X射线衍射技术在金属材料研究中的应用[J]. 中国材料进展, 2017, 36: 181)
[25] Sáfrán G."One-sample concept" micro-combinatory for high throughput TEM of binary films[J]. Ultramicroscopy, 2018, 187: 50
[26] Tsai P, Flores K M.A combinatorial strategy for metallic glass design via laser deposition[J]. Intermetallics, 2014, 55: 162
[27] Tsai P, Flores K M.A laser deposition strategy for the efficient identification of glass-forming alloys[J]. Metall. Mater. Trans., 2015, 46A: 3876
[28] Tsai P, Flores K M.High-throughput discovery and characterization of multicomponent bulk metallic glass alloys[J]. Acta Mater., 2016, 120: 426
[29] Wu H, Fan G H, Huang M, et al.Deformation behavior of brittle/ductile multilayered composites under interface constraint effect[J]. Int. J. Plast., 2017, 89: 96
[30] Onraet S, Luff D, Geers M, et al.Measurement of strain fields in the micron range [A]. 3rd International Micro Materials Conference and Poster Exhibition[C]. Berlin: Druckhaus Dresden GmbH, 2000: 578
[31] Muster T H, Trinchi A, Markley T A, et al.A review of high throughput and combinatorial electrochemistry[J]. Electrochim. Acta, 2011, 56: 9679
[32] Hanak J J.The "Multiple-Sample Concept" in materials research: Synthesis, compositional analysis and testing of entire multicomponent systems[J]. J. Mater. Sci., 1970, 5: 964
[33] Wang H Z, Wang H, Ding H, et al.Progress in high-throughput materials synthesis and characterization[J]. Sci. Technol. Rev., 2015, 33(10): 31)(王海舟, 汪洪, 丁洪等. 材料的高通量制备与表征技术[J]. 科技导报, 2015, 33(10): 31)
[34] Potyrailo R, Rajan K, Stoewe K, et al.Combinatorial and high-throughput screening of materials libraries: Review of state of the art[J]. ACS Comb. Sci., 2011, 13: 579
[35] Yoo Y K, Xue Q Z, Chu Y S, et al.Identification of amorphous phases in the Fe-Ni-Co ternary alloy system using continuous phase diagram material chips[J]. Intermetallics, 2006, 14: 241
[36] Takeuchi I, Chang K, Sharma R P, et al.Microstructural properties of (Ba, Sr)TiO3 films fabricated from BaF2/SrF2/TiO2 amorphous multilayers using the combinatorial precursor method[J]. J. Appl. Phys., 2001, 90: 2474
[37] Wang N, Zhang X, Chen B, et al.Microfluidic photoelectrocatalytic reactors for water purification with an integrated visible-light source[J]. Lab Chip, 2012, 12: 3983
[38] Bergh S, Guan S H, Hagemeyer A, et al.Gas phase oxidation of ethane to acetic acid using high-throughput screening in a massively parallel microfluidic reactor system[J]. Appl. Catal., 2003, 254A: 67
[39] Guram A, Hagemeyer A, Lugmair C G, et al.Application of high throughput screening to heterogeneous liquid and gas phase oxidation catalysis[J]. Adv. Synth. Catal., 2004, 346: 215
[40] Yan Z K, Zhang X K, Li G, et al.High-throughput combinatorial chemical bath deposition: The case of doping Cu(In, Ga)Se film with antimony[J]. Appl. Surf. Sci., 2018, 427: 1235
[41] Mao S S, Zhang X J.High-throughput multi-plume pulsed-laser deposition for materials exploration and optimization[J]. Engineering, 2015, 1: 367
[42] Fan H W, Shan L L, Meng H, et al.High-throughput production of nanodisperse hybrid membranes on various substrates[J]. J. Membr. Sci., 2018, 552: 177
[43] Wu H Y, Li J, Liu F, et al.A high-throughput methodology search for the optimum cooling rate in an advanced polycrystalline nickel base superalloy[J]. Mater. Des., 2017, 128: 176
[44] Goll D, Loeffler R, Hohs D, et al.Reaction sintering as a high-throughput approach for magnetic materials development[J]. Scr. Mater., 2018, 146: 355
[45] Ivanov R, Deschamps A, De Geuser F.High throughput evaluation of the effect of Mg concentration on natural ageing of Al-Cu-Li-(Mg) alloys[J]. Scr. Mater., 2018, 150: 156
[46] Chikyow T, Ahmet P, Nakajima K, et al.A combinatorial approach in oxide/semiconductor interface research for future electronic devices[J]. Appl. Surf. Sci., 2002, 189: 284
[47] Baufeld B, Van Der Biest O, Gault R. Additive manufacturing of Ti-6Al-4V components by shaped metal deposition: Microstructure and mechanical properties[J]. Mater. Des., 2010, 31(suppl.1): S106
[48] Schwendner K I, Banerjee R, Collins P C, et al.Direct laser deposition of alloys from elemental powder blends[J]. Scr. Mater., 2001, 45: 1123
[49] Arnold C B, Serra P, Piqué A.Laser direct-write techniques for printing of complex materials[J]. MRS Bull., 2007, 32: 23
[50] Nian Q, Wang Y, Yang Y, et al.Direct laser writing of nanodiamond films from graphite under ambient conditions[J]. Sci. Rep., 2015, 4: 6612
[51] Zygmuntowicz J, Wiecińska P, Miazga A, et al.Al2O3/Ni functionally graded materials (FGM) obtained by centrifugal-slip casting method[J]. J. Therm. Anal. Calorim., 2017, 130: 123
[52] Solarek J, Aneziris C G, Biermann H.A new method for manufacturing graded refractories by localized hot uniaxial pressing[J]. Ceram. Int., 2017, 43: 14636
[53] Avci U, Temiz ?.A new approach to the production of partially graded and laminated composite material composed of SiC-reinforced 7039 Al alloy plates at different rates[J]. Composites, 2017, 131B: 76
[54] Cai Y Z, Cheng L F, Yin H F, et al.Preparation and mechanical properties of Ti3SiC2/SiC functionally graded materials[J]. Ceram. Int., 2017, 43: 6648
[55] Shishkovsky I, Kakovkina N, Sherbakov V.Graded layered titanium composite structures with TiB2 inclusions fabricated by selective laser melting[J]. Compos. Struct., 2017, 169: 90
[56] Uchic M D, Dimiduk D M. A methodology to investigate size scale effects in crystalline plasticity using uniaxial compression testing [J]. Mater. Sci. Eng., 2005, A400-401: 268
[57] Guo X L, Guo Q, Li Z Q, et al.Size and crystallographic orientation effects on the mechanical behavior of 4H-SiC micro-/nano-pillars[J]. Metall. Mater. Trans., 2018, 49A: 439
[58] Deng C F, Zhang X X, Wang D Z.Chemical stability of carbon nanotubes in the 2024Al matrix[J]. Mater. Lett., 2007, 61: 904
[59] Li J C, Zhang X X, Geng L.Improving graphene distribution and mechanical properties of GNP/Al composites by cold drawing[J]. Mater. Des., 2018, 144: 159
[60] Huang L J, Geng L, Fu Y, et al.Oxidation behavior of in situ TiCp/Ti6Al4V composite with self-assembled network microstructure fabricated by reaction hot pressing[J]. Corros. Sci., 2013, 69: 175
[61] Huang L J, Wang S, Geng L, et al.Low volume fraction in situ (Ti5Si3+Ti2C)/Ti hybrid composites with network microstructure fabricated by reaction hot pressing of Ti-SiC system[J]. Compos. Sci. Technol., 2013, 82: 23
[62] Huang M, Xu C, Fan G H, et al.Role of layered structure in ductility improvement of layered Ti-Al metal composite[J]. Acta Mater., 2018, 153: 235
[63] Wu H, Fan G H, Jin B C, et al.Fabrication and mechanical properties of TiBw/Ti-Ti(Al) laminated composites[J]. Mater. Des., 2016, 89: 697
[64] Collins F S, Morgan M, Patrinos A.The human genome project: Lessons from large-scale biology[J]. Science, 2003, 300: 286
[65] Isaacs E D, Marcus M, Aeppli G, et al.Synchrotron X-ray microbeam diagnostics of combinatorial synthesis[J]. Appl. Phys. Lett., 1998, 73: 1820
[66] Picos-Vega A, Ramírez-Bon R, Espinoza-Beltrán F J, et al. Physical properties of CdTe-Sb thin films [J]. Thin Solid Films, 1996, 290-291: 395
[67] Jiang R Z, Chu D.A combinatorial approach toward electrochemical analysis[J]. J. Electroanal. Chem., 2002, 527: 137
[68] Mardare A I, Yadav A P, Wieck A D, et al.Combinatorial electrochemistry on Al-Fe alloys[J]. Sci. Technol. Adv. Mater., 2016, 9: 035009
[69] Hassel A W, Lohrengel M M.The scanning droplet cell and its application to structured nanometer oxide films on aluminium[J]. Electrochim. Acta, 1997, 42: 3327
[70] Vegas A J, Anderson D G.High-throughput approaches[J]. Polym. Sci., 2012, 9A: 457
[71] Urquhart A J, Anderson D G, Taylor M, et al.High throughput surface characterisation of a combinatorial material library[J]. Adv. Mater., 2007, 19: 2486
[72] Orikasa Y, Maeda T, Koyama Y, et al.Direct observation of a metastable crystal phase of LixFePO4 under electrochemical phase transition[J]. J. Am. Chem. Soc., 2013, 135: 5497
[73] Zhou Y N, Yue J L, Hu E Y, et al.High-rate charging induced intermediate phases and structural changes of layer-structured cathode for lithium-ion batteries[J]. Adv. Energy Mater., 2016, 6: 1600597
[74] Lyu Y, Liu Y L, Cheng T, et al.High-throughput characterization methods for lithium batteries[J]. J. Mater., 2017, 3: 221
[75] Meirer F, Cabana J, Liu Y, et al.Three-dimensional imaging of chemical phase transformations at the nanoscale with full-field transmission X-ray microscopy[J]. J. Synchrotron Radiat., 2011, 18: 773
[76] Li S Y, Beyerlein I J, Alexander D J, et al.Texture evolution during multi-pass equal channel angular extrusion of copper: Neutron diffraction characterization and polycrystal modeling[J]. Acta Mater., 2005, 53: 2111
[77] Pouillerie C, Suard E, Delmas C.Structural characterization of Li1-z-xNi1+zO2 by neutron diffraction[J]. J. Solid State Chem., 2001, 158: 187
[78] Thibault D, Bocher P, Thomas M, et al.Residual stress characterization in low transformation temperature 13%Cr-4%Ni stainless steel weld by neutron diffraction and the contour method[J]. Mater. Sci. Eng., 2010, A527: 6205
[79] Wei T, Xiang X D, Wallace-Freedman W G, et al. Scanning tip microwave near-field microscope[J]. Appl. Phys. Lett., 1996, 68: 3506
[80] Gao C, Duewer F, Xiang X D.Quantitative microwave evanescent microscopy[J]. Appl. Phys. Lett., 1999, 75: 3005
[81] Oguchi H, Heilweil E J, Josell D, et al.Infrared emission imaging as a tool for characterization of hydrogen storage materials[J]. J. Alloys Compd., 2009, 477: 8
[82] Weiss P A W, Thome C, Maier W F. MS-Express: Data-extracting and -processing software for high-throughput experimentation with mass spectrometry[J]. J. Comb. Chem., 2004, 6: 520
[83] Hoffmann C, Schmidt H W, Schüth F.A multipurpose parallelized 49-channel reactor for the screening of catalysts: Methane oxidation as the example reaction[J]. J. Catal., 2001, 198: 348
[84] Sottmann J, Homs-Regojo R, Wragg D S, et al.Versatile electrochemical cell for Li/Na-ion batteries and high-throughput setup for combined operando X-ray diffraction and absorption spectroscopy[J]. J Appl. Crystallogr., 2016, 49: 1972
[85] Zhang X K, Xiang Y.Combinatorial approaches for high-throughput characterization of mechanical properties[J]. J. Mater., 2017, 3: 209
[86] Shapiro M J, Gounarides J S.NMR methods utilized in combinatorial chemistry research[J]. Prog. Nucl. Magn. Reson. Spectrosc., 1999, 35: 153
[87] Blümich B, Casanova F, Appelt S.NMR at low magnetic fields[J]. Chem. Phys. Lett., 2009, 477: 231
[88] Johann T, Brenner A, Schwickardi M, et al.Listening to catalysis—A real time parallel method for high throughput product analysis[J]. Catal. Today, 2003, 81: 449
[89] Meersschaut J, Vandervorst W.High-throughput ion beam analysis at imec[J]. Nucl. Instrum. Meth. Phys. Res., 2017, 406B: 25
[90] Rudneva M, Kozlova T, Zandbergen H W.New possibilities for in-situ electrical characterization of nanosamples at different temperatures combined with simultaneous TEM observations[J]. Microsc. Microanal., 2013, 19(suppl.2): 456
[91] Levine L E, Larson B C, Yang W G, et al.X-ray microbeam measurements of individual dislocation cell elastic strains in deformed single-crystal copper[J]. Nat. Mater., 2006, 5: 619
[92] Nix W D, Gao H J.Indentation size effects in crystalline materials: A law for strain gradient plasticity[J]. J. Mech. Phys. Solids, 1998, 46: 411
[93] Hutchinson J W.Plasticity at the micron scale[J]. Int. J. Solids Struct., 2000, 37: 225
[94] Tymiak N I, Kramer D E, Bahr D F, et al.Plastic strain and strain gradients at very small indentation depths[J]. Acta Mater., 2001, 49: 1021
[95] Su H, Yeung E S.High-throughput screening of heterogeneous catalysts by laser-induced fluorescence imaging[J]. J. Am. Chem. Soc., 2000, 122: 7422
[96] Vogt S, Chu Y S, Tkachuk A, et al.Composition characterization of combinatorial materials by scanning X-ray fluorescence microscopy using microfocused synchrotron X-ray beam[J]. Appl. Surf. Sci., 2004, 223: 214
[97] Linke S, Kühn J, N?rthemann K, et al.Sensor high throughput screening using photocurrent measurements in silicon[J]. Proc. Eng., 2012, 47: 1195
[98] Chen Y H, Yuan L J, Wang H Z.Investigation on original statistic distribution analysis of flat-bulb steel by laser ablation inductively coupled plasma mass spectrometry[J]. Metall. Anal., 2008, 29(9): 1(陈玉红, 袁良经, 王海舟. 球扁钢的激光剥蚀-电感耦合等离子体质谱原位统计分布分析研究[J]. 冶金分析, 2008, 29(9): 1)
[99] Wang H Z.In situ statistical distribution analysis—A new technique for materials research and quality criterion[J]. Sci. China, 2002, 32B: 481(王海舟. 原位统计分布分析——材料研究及质量判据的新技术[J]. 中国科学, 2002, 32B: 481)
[100] Li D L, Wang H Z.Original Position statistic distribution analysis for the sulfides in gear steels[J]. ISIJ Int., 2014, 54: 160
[101] Luo Q H, Li D L, Ma F C, et al.Original position statistic distribution analysis for inclusion of cross-section of stainless steel continuous casting slab[J]. Metall. Anal., 2013, 33(12): 1(罗倩华, 李冬玲, 马飞超 等. 不锈钢连铸板坯横截面夹杂物的原位统计分布分析 [J]. 冶金分析, 2013, 33(12): 1)
[102] Huang X X, Wu G L, Zhong X Y, et al.Multi-scale and multi-dimensional characterization techniques for advanced materials[J]. J. Chin. Electr. Microsc. Soc., 2016, 35: 567(黄晓旭, 吴桂林, 钟虓 等. 先进材料多维多尺度高通量表征技术[J]. 电子显微学报, 2016, 35: 567)
[103] Gao C, Xiang X D.Quantitative microwave near-field microscopy of dielectric properties[J]. Rev. Sci. Instrum., 1998, 69: 3846
[104] Ohtani M, Lippmaa M, Ohnishi T, et al.High throughput oxide lattice engineering by parallel laser molecular-beam epitaxy and concurrent X-ray diffraction[J]. Rev. Sci. Instrum., 2005, 76: 062218
[105] Nam K W, Bak S M, Hu E Y, et al.Cathode Materials: Combining in situ synchrotron X-Ray diffraction and absorption techniques with transmission electron microscopy to study the origin of thermal instability in overcharged cathode materials for lithium-ion batteries[J]. Adv. Funct. Mater., 2013, 23: 1046
[106] Zheng X, Cahill D G, Weaver R, et al.Micron-scale measurements of the coefficient of thermal expansion by time-domain probe beam deflection[J]. J. Appl. Phys., 2008, 104: 0735097
[1] 马国楠, 朱士泽, 王东, 肖伯律, 马宗义. SiC颗粒增强Al-Zn-Mg-Cu复合材料的时效行为和力学性能[J]. 金属学报, 2023, 59(12): 1655-1664.
[2] 范根莲, 郭峙岐, 谭占秋, 李志强. 金属材料的构型化复合与强韧化[J]. 金属学报, 2022, 58(11): 1416-1426.
[3] 朱士泽, 王东, 王全兆, 肖伯律, 马宗义. Cu含量对SiC/Al-Mg-Si-Cu复合材料自然时效负面效应的影响[J]. 金属学报, 2021, 57(7): 928-936.
[4] 钱漪, 袁广银. 可降解锌合金血管支架的研究现状、面临的挑战与对策思考[J]. 金属学报, 2021, 57(3): 272-282.
[5] 赵雷, 王辉, 杨丽霞, 陈学斌, 郎润秋, 贺林峰, 陈东风, 王海舟. Fe-Co-Ni系组合合金热等静压高通量制备方法初探[J]. 金属学报, 2021, 57(12): 1627-1636.
[6] 刘东雷, 陈情, 王德, 张睿, 王文琴. Ti-6Al-4V表面电子束熔覆(Ti, W)C1-x复合涂层的形成及摩擦性能[J]. 金属学报, 2020, 56(7): 1025-1035.
[7] 马国楠, 王东, 刘振宇, 毕胜, 昝宇宁, 肖伯律, 马宗义. 热压烧结温度对SiC/Al-Zn-Mg-Cu复合材料微观结构与力学性能的影响[J]. 金属学报, 2019, 55(10): 1319-1328.
[8] 肖伯律, 黄治冶, 马凯, 张星星, 马宗义. 非连续增强铝基复合材料的热变形行为研究进展[J]. 金属学报, 2019, 55(1): 59-72.
[9] 武高辉, 乔菁, 姜龙涛. Al及其复合材料尺寸稳定性原理与稳定化设计研究进展[J]. 金属学报, 2019, 55(1): 33-44.
[10] 范同祥, 刘悦, 杨昆明, 宋健, 张荻. 碳/金属复合材料界面结构优化及界面作用机制的研究进展[J]. 金属学报, 2019, 55(1): 16-32.
[11] 王艳秋,吴昆,王福会. 第二相对镁基材料微弧氧化过程的影响机制*[J]. 金属学报, 2016, 52(6): 689-697.
[12] 许世娇 肖伯律 刘振宇 王文广 马宗义. 高能球磨法制备的碳纳米管增强铝基复合材料的微观组织和力学性能[J]. 金属学报, 2012, 48(7): 882-888.
[13] 顾冬冬; 沈以赴 . 添加La2O3对激光烧结(WC-Co)p/Cu金属基复合材料组织和成形性能的影响[J]. 金属学报, 2007, 43(9): 968-976 .
[14] 郭素娟; 康国政 . SiCp/6061Al合金复合材料循环变形行为的有限元模拟[J]. 金属学报, 2006, 42(10): 1051-1055 .
[15] 李斌; 许庆彦; 李旭东; 柳百成 . 用颗粒推移模型模拟Al-Si/SiCp复合材料微观组织[J]. 金属学报, 2005, 41(12): 1303-1308 .