Please wait a minute...
金属学报  2026, Vol. 62 Issue (5): 743-755    DOI: 10.11900/0412.1961.2025.00322
  综述 本期目录 | 过刊浏览 |
面向极端服役条件的高熵合金结构材料:性能优势、瓶颈与突破路径
吕昭平(), 申耀祖, 王先珍, 陈强, 唐建国, 张晓宾, 于勇, 蒋虽合, 刘雄军, 王辉, 吴渊
北京科技大学 新金属材料全国重点实验室 北京 100083
High-Entropy Alloys in Extreme Environments: A Perspective on Advantages, Challenges, and Breakthroughs
LU Zhaoping(), SHEN Yaozu, WANG Xianzhen, CHEN Qiang, TANG Jianguo, ZHANG Xiaobin, YU Yong, JIANG Suihe, LIU Xiongjun, WANG Hui, WU Yuan
State Key Laboratory for Advanced Metals and Materials, University of Science and Technology Beijing, Beijing 100083, China
引用本文:

吕昭平, 申耀祖, 王先珍, 陈强, 唐建国, 张晓宾, 于勇, 蒋虽合, 刘雄军, 王辉, 吴渊. 面向极端服役条件的高熵合金结构材料:性能优势、瓶颈与突破路径[J]. 金属学报, 2026, 62(5): 743-755.
Zhaoping LU, Yaozu SHEN, Xianzhen WANG, Qiang CHEN, Jianguo TANG, Xiaobin ZHANG, Yong YU, Suihe JIANG, Xiongjun LIU, Hui WANG, Yuan WU. High-Entropy Alloys in Extreme Environments: A Perspective on Advantages, Challenges, and Breakthroughs[J]. Acta Metall Sin, 2026, 62(5): 743-755.

全文: PDF(2963 KB)   HTML
摘要: 

超高温、极低温和强辐照是航空、航天、核能和深海装备等在服役过程中面临的极端工况。传统单一主元合金因相稳定性不足、低温韧脆转变及缺陷演化失控,性能已逼近极限,成为制约高端装备升级的核心瓶颈。高熵合金凭借多主元耦合的高构型熵、晶格畸变和化学短程有序,在极端条件下具有高热-力学稳定性、优异低温韧塑性和抗辐照损伤能力,被视为最具突破性能边界潜力的合金体系。本文系统梳理了高熵合金作为极端环境结构材料的潜力和挑战,围绕超高温、极低温和强辐照三类典型场景,剖析其性能优势并揭示高熵效应的作用机制。最后,总结关键瓶颈并提出发展路径,为高熵合金从实验室走向工程应用提供参考。

关键词 : 高熵合金,  极端服役条件,  结构材料,  力学性能    
Abstract:

Extreme environments, such as ultra-high temperatures, extremely low temperatures, and intense irradiation, impose growing demands on structural materials for next-generation engineering applications. Conventional single-principal-element alloys are approaching their performance limits because of insufficient phase stability, low-temperature ductile-to-brittle transitions, and uncontrolled defect evolution. Conversely, high-entropy alloys (HEAs), characterized by multi-principal elements, exhibit high configurational entropy, severe lattice distortion, and chemical short-range order. These intrinsic characteristics enable exceptional thermal-mechanical stability, cryogenic toughness, and irradiation resistance, rendering them promising candidates for applications in extreme environments. Focusing on three representative conditions, this work summarizes the potentials and challenges of HEAs as structural materials, clarifies the underlying high-entropy-driven mechanisms, and identifies key technological barriers. Furthermore, we report perspectives on future research directions and propose pathways to accelerate the transition of HEAs from laboratory-scale research to practical engineering applications.

Key words: high-entropy alloy    extreme environment    structural material    mechanical property
收稿日期: 2025-10-15     
ZTFLH:  TG139  
基金资助:国家自然科学基金项目(52201171);国家自然科学基金项目(52225103);国家自然科学基金项目(52322102);国家自然科学基金项目(U2441262);国家自然科学基金项目(W2412068);国家重点研发计划项目(2022-YFB4602101);中央高校基本科研业务费项目(FRF-IDRY-23-020);新金属材料全国重点实验室自主研究课题项目(2025-S11)
通讯作者: 吕昭平,luzp@ustb.edu.cn,主要从事非晶与高熵合金、高性能钢铁等材料的高效设计与结构-性能关联研究
Corresponding author: LU Zhaoping, professor, Tel: (010)82375387, E-mail: luzp@ustb.edu.cn
作者简介: 吕昭平,男,1970年生,教授,博士,中国科学院院士
图1  不同高温结构材料的屈服强度-温度汇总[24]
图2  通过晶界工程策略实现超高温难熔高熵合金室温塑性与超高温强度的协同提升[31]
图3  通过引入共晶碳化物实现超高温难熔高熵合金室温/高温力学性能的协同提升[42]
图4  CrCoNi合金的低温断裂韧性及变形组织分析[47]
图5  HfNbTaTiZr高熵合金室温和低温下的工程应力-应变曲线及变形机制分析[56]
图6  主元数量对合金中空洞等辐照缺陷的影响[65]
图7  局域化学有序结构和成分波动对高熵合金中辐照缺陷的影响[74]
[1] Yeh J W, Chen S K, Lin S J, et al. Nanostructured high-entropy alloys with multiple principal elements: Novel alloy design concepts and outcomes [J]. Adv. Eng. Mater., 2004, 6: 299
doi: 10.1002/adem.v6:5
[2] Cantor B, Chang I T H, Knight P, et al. Microstructural development in equiatomic multicomponent alloys [J]. Mater. Sci. Eng., 2004, A375-377: 213
[3] Senkov O N, Miller J D, Miracle D B, et al. Accelerated exploration of multi-principal element alloys with solid solution phases [J]. Nat. Commun., 2015, 6: 6529
doi: 10.1038/ncomms7529 pmid: 25739749
[4] Senkov O N, Wilks G B, Scott J M, et al. Mechanical properties of Nb25Mo25Ta25W25 and V20Nb20Mo20Ta20W20 refractory high entropy alloys [J]. Intermetallics, 2011, 19: 698
doi: 10.1016/j.intermet.2011.01.004
[5] Han J C, Song B, Xu P, et al. Multiscale synthesis and performance regulation mechanisms of high-entropy materials [J]. Acta Metall Sin, 2026, 62: 397
doi: 10.11900/0412.1961.2025.00405
[5] 韩杰才, 宋 波, 徐 平 等. 高熵材料的多尺度制备及性能调控机制 [J]. 金属学报, 2026, 62: 397
doi: 10.11900/0412.1961.2025.00405
[6] Senkov O N, Scott J M, Senkova S V, et al. Microstructure and room temperature properties of a high-entropy TaNbHfZrTi alloy [J]. J. Alloys Compd., 2011, 509: 6043
doi: 10.1016/j.jallcom.2011.02.171
[7] George E P, Raabe D, Ritchie R O. High-entropy alloys [J]. Nat. Rev. Mater., 2019, 4: 515
doi: 10.1038/s41578-019-0121-4
[8] Wu Y, Zhang F, Yuan X Y, et al. Short-range ordering and its effects on mechanical properties of high-entropy alloys [J]. J. Mater. Sci. Technol., 2021, 62: 214
doi: 10.1016/j.jmst.2020.06.018
[9] Wang Y H, Jiao M Y, Wu Y, et al. Enhancing properties of high-entropy alloys via manipulation of local chemical ordering [J]. J. Mater. Sci. Technol., 2024, 180: 23
doi: 10.1016/j.jmst.2023.10.003
[10] Han X D, An Z B, Mao S H, et al. Negative mixing enthalpy alloying to promote the development of alloys with high strength and ductility [J]. Acta Metall. Sin., 2025, 61: 953
doi: 10.11900/0412.1961.2025.00153
[10] 韩晓东, 安子冰, 毛圣成 等. 负混合焓合金化推动高强韧合金发展 [J]. 金属学报, 2025, 61: 953
doi: 10.11900/0412.1961.2025.00153
[11] Jiao M Y, Lei Z F, Wu Y, et al. Manipulating the ordered oxygen complexes to achieve high strength and ductility in medium-entropy alloys [J]. Nat. Commun., 2023, 14: 806
doi: 10.1038/s41467-023-36319-0 pmid: 36781880
[12] Ma E, Liu C. Achieving alloys with concurrent high strength and high ductility [J]. Acta Metall. Sin., 2025, 61: 665
doi: 10.11900/0412.1961.2024.00422
[12] 马 恩, 刘 畅. 如何使合金兼具高强度与高塑性 [J]. 金属学报, 2025, 61: 665
[13] Eswarappa Prameela S, Pollock T M, Raabe D, et al. Materials for extreme environments [J]. Nat. Rev. Mater., 2023, 8: 81
doi: 10.1038/s41578-022-00496-z
[14] Han L L, Zhu S Y, Rao Z Y, et al. Multifunctional high-entropy materials [J]. Nat. Rev. Mater., 2024, 9: 846
doi: 10.1038/s41578-024-00720-y
[15] Qi H, Chen L, Deng S Q, et al. High-entropy ferroelectric materials [J]. Nat. Rev. Mater., 2023, 8: 355
doi: 10.1038/s41578-023-00544-2
[16] Yang T, Zhao Y L, Tong Y, et al. Multicomponent intermetallic nanoparticles and superb mechanical behaviors of complex alloys [J]. Science, 2018, 362: 933
doi: 10.1126/science.aas8815 pmid: 30467166
[17] Lee C, Song G, Gao M C, et al. Lattice distortion in a strong and ductile refractory high-entropy alloy [J]. Acta Mater., 2018, 160: 158
doi: 10.1016/j.actamat.2018.08.053
[18] Chen H, Xu Y J, Liu L H, et al. Lattice distortion tuning resistivity Invar effect in high-entropy alloys [J]. Phys. Rev., 2025, 111B: 094209
[19] Lei Z F, Liu X J, Wu Y, et al. Enhanced strength and ductility in a high-entropy alloy via ordered oxygen complexes [J]. Nature, 2018, 563: 546
doi: 10.1038/s41586-018-0685-y
[20] Ding J, Yu Q, Asta M, et al. Tunable stacking fault energies by tailoring local chemical order in CrCoNi medium-entropy alloys [J]. Proc. Natl. Acad. Sci. U.S.A., 2018, 115: 8919
doi: 10.1073/pnas.1808660115 pmid: 30127034
[21] Perepezko J H. The hotter the engine, the better [J]. Science, 2009, 326: 1068
doi: 10.1126/science.1179327 pmid: 19965415
[22] Zhao J C, Westbrook J H. Ultrahigh-temperature materials for jet engines [J]. MRS Bull., 2003, 28: 622
doi: 10.1557/mrs2003.189
[23] Senkov O N, Miracle D B, Chaput K J, et al. Development and exploration of refractory high entropy alloys—A review [J]. J. Mater. Res., 2018, 33: 3092
doi: 10.1557/jmr.2018.153
[24] Shen Y Z, Wang X Z, Zhang X B, et al. Research progress on mechanical properties of ultra-high temperature WTa-containing refractory multi-principal element alloys [J]. Tungsten, 2025, 7: 680
doi: 10.1007/s42864-025-00324-1
[25] Chen B, Li S Z, Ding J, et al. Correlating dislocation mobility with local lattice distortion in refractory multi-principal element alloys [J]. Scr. Mater., 2023, 222: 115048
doi: 10.1016/j.scriptamat.2022.115048
[26] Wang X Y, Maresca F, Cao P H. The hierarchical energy landscape of screw dislocation motion in refractory high-entropy alloys [J]. Acta Mater., 2022, 234: 118022
doi: 10.1016/j.actamat.2022.118022
[27] Maresca F, Curtin W A. Mechanistic origin of high strength in refractory BCC high entropy alloys up to 1900 K [J]. Acta Mater., 2020, 182: 235
doi: 10.1016/j.actamat.2019.10.015
[28] Yin S, Zuo Y X, Abu-Odeh A, et al. Atomistic simulations of dislocation mobility in refractory high-entropy alloys and the effect of chemical short-range order [J]. Nat. Commun., 2021, 12: 4873
doi: 10.1038/s41467-021-25134-0 pmid: 34381027
[29] Tsuru T, Han S, Matsuura S, et al. Intrinsic factors responsible for brittle versus ductile nature of refractory high-entropy alloys [J]. Nat. Commun., 2024, 15: 1706
doi: 10.1038/s41467-024-45639-8 pmid: 38402252
[30] Belcher C H, MacDonald B E, Apelian D, et al. The role of interstitial constituents in refractory complex concentrated alloys [J]. Prog. Mater. Sci., 2023, 137: 101140
doi: 10.1016/j.pmatsci.2023.101140
[31] Wang Z Q, Wu H H, Wu Y, et al. Solving oxygen embrittlement of refractory high-entropy alloy via grain boundary engineering [J]. Mater. Today, 2022, 54: 83
doi: 10.1016/j.mattod.2022.02.006
[32] Han Z D, Luan H W, Liu X, et al. Microstructures and mechanical properties of Ti x NbMoTaW refractory high-entropy alloys [J]. Mater. Sci. Eng., 2018, A712: 380
[33] Li T X, Jiao W N, Miao J W, et al. A novel ZrNbMoTaW refractory high-entropy alloy with in-situ forming heterogeneous structure [J]. Mater. Sci. Eng., 2021, A827: 142061
[34] Sun Y P, Hou C, Li Y R, et al. Ultrafine-grained refractory high-entropy alloy with oxygen control and high mechanical performance [J]. J. Mater. Sci. Technol., 2025, 215: 45
doi: 10.1016/j.jmst.2024.07.017
[35] Golla B R, Mukhopadhyay A, Basu B, et al. Review on ultra-high temperature boride ceramics [J]. Prog. Mater. Sci., 2020, 111: 100651
doi: 10.1016/j.pmatsci.2020.100651
[36] Wei Q Q, Xu X D, Shen Q, et al. Metal-carbide eutectics with multiprincipal elements make superrefractory alloys [J]. Sci. Adv., 2022, 8: eabo2068
doi: 10.1126/sciadv.abo2068
[37] Wan Y X, Wang X, Zhang Z B, et al. Structures and properties of the (NbMoTaW)100 - x C x high-entropy composites [J]. J. Alloys Compd., 2021, 889: 161645
doi: 10.1016/j.jallcom.2021.161645
[38] Wu S Y, Qiao D X, Zhang H T, et al. Microstructure and mechanical properties of C x Hf0.25NbTaW0.5 refractory high-entropy alloys at room and high temperatures [J]. J. Mater. Sci. Technol., 2022, 97: 229
doi: 10.1016/j.jmst.2021.05.015
[39] Wei Q Q, Luo G Q, Zhang J, et al. Designing high entropy alloy-ceramic eutectic composites of MoNbRe0.5TaW(TiC) x with high compressive strength [J]. J. Alloys Compd., 2020, 818: 152846
doi: 10.1016/j.jallcom.2019.152846
[40] He H T, Wang J X, Cao Y, et al. Effect of Re and C on mechanical properties of NbTaW0.4 refractory medium-entropy alloy at elevated temperature [J]. J. Alloys Compd., 2023, 931: 167421
doi: 10.1016/j.jallcom.2022.167421
[41] Wu S Y, Qiao D X, Zhao H L, et al. A novel NbTaW0.5 (Mo2C) x refractory high-entropy alloy with excellent mechanical properties [J]. J. Alloys Compd., 2021, 889: 161800
doi: 10.1016/j.jallcom.2021.161800
[42] Shen Y Z, Wang Z Q, Wang X Z, et al. Enhancing mechanical properties of refractory multi-principal element alloys via compositionally complex carbides [J]. J. Mater. Sci. Technol., 2025, 232: 191
doi: 10.1016/j.jmst.2025.03.001
[43] Tanaka M, Tarleton E, Roberts S G. The brittle-ductile transition in single-crystal iron [J]. Acta Mater., 2008, 56: 5123
doi: 10.1016/j.actamat.2008.06.025
[44] Liu J P, Chen H, Zhang C, et al. Progress of cryogenic deformation and strengthening-toughening mechanisms of high-entropy alloys [J]. Acta Metall. Sin., 2023, 59: 727.
doi: 10.11900/0412.1961.2022.00598
[44] 刘俊鹏, 陈 浩, 张 弛 等. 高熵合金的低温塑性变形机制及强韧化研究进展 [J]. 金属学报, 2023, 59: 727
doi: 10.11900/0412.1961.2022.00598
[45] Gludovatz B, Hohenwarter A, Catoor D, et al. A fracture-resistant high-entropy alloy for cryogenic applications [J]. Science, 2014, 345: 1153
doi: 10.1126/science.1254581 pmid: 25190791
[46] Gludovatz B, Hohenwarter A, Thurston K V S, et al. Exceptional damage-tolerance of a medium-entropy alloy CrCoNi at cryogenic temperatures [J]. Nat. Commun., 2016, 7: 10602
doi: 10.1038/ncomms10602 pmid: 26830651
[47] Liu D, Yu Q, Kabra S, et al. Exceptional fracture toughness of CrCoNi-based medium- and high-entropy alloys at 20 kelvin [J]. Science, 2022, 378: 978
doi: 10.1126/science.abp8070 pmid: 36454850
[48] Jo Y H, Jung S, Choi W M, et al. Cryogenic strength improvement by utilizing room-temperature deformation twinning in a partially recrystallized VCrMnFeCoNi high-entropy alloy [J]. Nat. Commun., 2017, 8: 15719
doi: 10.1038/ncomms15719 pmid: 28604656
[49] Seol J B, Bae J W, Kim J G, et al. Short-range order strengthening in boron-doped high-entropy alloys for cryogenic applications [J]. Acta Mater., 2020, 194: 366
doi: 10.1016/j.actamat.2020.04.052
[50] Lu Y P, Gao X Z, Jiang L, et al. Directly cast bulk eutectic and near-eutectic high entropy alloys with balanced strength and ductility in a wide temperature range [J]. Acta Mater., 2017, 124: 143
doi: 10.1016/j.actamat.2016.11.016
[51] Sung M Y, Jang T J, Song S Y, et al. Ultrahigh strength with suppressed flow instability at liquid helium temperature via coherent nanoprecipitation in a medium-entropy alloy [J]. Adv. Funct. Mater., 2025, 36: e15593
doi: 10.1002/adfm.v36.10
[52] Wang F, Song M, Elkot M N, et al. Shearing brittle intermetallics enhances cryogenic strength and ductility of steels [J]. Science, 2024, 384: 1017
doi: 10.1126/science.ado2919 pmid: 38815014
[53] Yang T, Zhao Y L, Luan J H, et al. Nanoparticles-strengthened high-entropy alloys for cryogenic applications showing an exceptional strength-ductility synergy [J]. Scr. Mater., 2019, 164: 30
doi: 10.1016/j.scriptamat.2019.01.034
[54] Sohail Y, Zhang C L, Gao S H, et al. A complex concentrated alloy with record-high strength-toughness at 77 K [J]. Adv. Mater., 2025, 37: 2410923.
doi: 10.1002/adma.v37.4
[55] Lu T W, Sun B H, Li Y, et al. Dual-scale chemical ordering for cryogenic properties in CoNiV-based alloys [J]. Nature, 2025, 645: 385
doi: 10.1038/s41586-025-09458-1
[56] Wang S B, Wu M X, Shu D, et al. Mechanical instability and tensile properties of TiZrHfNbTa high entropy alloy at cryogenic temperatures [J]. Acta Mater., 2020, 201: 517
doi: 10.1016/j.actamat.2020.10.044
[57] Wen X C, Wu Y, Huang H L, et al. Effects of Nb on deformation-induced transformation and mechanical properties of HfNbxTa0.2-TiZr high entropy alloys [J]. Mater. Sci. Eng., 2021, A805: 140798
[58] Cook D H, Kumar P, Payne M I, et al. Kink bands promote exceptional fracture resistance in a NbTaTiHf refractory medium-entropy alloy [J]. Science, 2024, 384: 178
doi: 10.1126/science.adn2428 pmid: 38603511
[59] Zinkle S J, Was G S. Materials challenges in nuclear energy [J]. Acta Mater., 2013, 61: 735
doi: 10.1016/j.actamat.2012.11.004
[60] Murty K L, Charit I. Structural materials for Gen-IV nuclear reactors: Challenges and opportunities [J]. J. Nucl. Mater., 2008, 383: 189
doi: 10.1016/j.jnucmat.2008.08.044
[61] Johnston W G, Rosolowski J H, Turkalo A M, et al. An experimental survey of swelling in commercial Fe-Cr-Ni alloys bombarded with 5 MeV Ni ions [J]. J. Nucl. Mater., 1974, 54: 24
doi: 10.1016/0022-3115(74)90073-7
[62] Nagase T, Rack P D, Noh J H, et al. In-situ TEM observation of structural changes in nano-crystalline CoCrCuFeNi multicomponent high-entropy alloy (HEA) under fast electron irradiation by high voltage electron microscopy (HVEM) [J]. Intermetallics, 2015, 59: 32
doi: 10.1016/j.intermet.2014.12.007
[63] Zhang Y W, Stocks G M, Jin K, et al. Influence of chemical disorder on energy dissipation and defect evolution in concentrated solid solution alloys [J]. Nat. Commun., 2015, 6: 8736
doi: 10.1038/ncomms9736 pmid: 26507943
[64] Granberg F, Nordlund K, Ullah M W, et al. Mechanism of radiation damage reduction in equiatomic multicomponent single phase alloys [J]. Phys. Rev. Lett., 2016, 116: 135504
doi: 10.1103/PhysRevLett.116.135504
[65] Lu C Y, Niu L L, Chen N J, et al. Enhancing radiation tolerance by controlling defect mobility and migration pathways in multicomponent single-phase alloys [J]. Nat. Commun., 2016, 7: 13564
doi: 10.1038/ncomms13564 pmid: 27976669
[66] Li D, Jia N, Huang H, et al. Helium ion irradiation enhanced precipitation and the impact on cavity formation in a HfNbZrTi refractory high entropy alloy [J]. J. Nucl. Mater., 2021, 552: 153023
doi: 10.1016/j.jnucmat.2021.153023
[67] Xia X C, Zhang E K, Ding J, et al. Research progress on laser cladding of refractory high-entropy alloy coatings [J]. Acta Metall Sin, 2025, 61: 59
doi: 10.11900/0412.1961.2024.00146
[67] 夏兴川, 张恩宽, 丁 俭 等. 激光熔覆难熔高熵合金涂层研究进展 [J]. 金属学报, 2025, 61: 59
doi: 10.11900/0412.1961.2024.00146
[68] Jin K, Bei H B. Single-phase concentrated solid-solution alloys: Bridging intrinsic transport properties and irradiation resistance [J]. Front. Mater., 2018, 5: 26
doi: 10.3389/fmats.2018.00026
[69] Jin K, Zhang C, Zhang F, et al. Influence of compositional complexity on interdiffusion in Ni-containing concentrated solid-solution alloys [J]. Mater. Res. Lett., 2018, 6: 293
doi: 10.1080/21663831.2018.1446466
[70] Zhao S J, Egami T, Stocks G M, et al. Effect of d electrons on defect properties in equiatomic NiCoCr and NiCoFeCr concentrated solid solution alloys [J]. Phys. Rev. Mater., 2018, 2: 013602
[71] Ding J, Wang Z J. Local chemical order in high-entropy alloys [J]. Acta Metall Sin, 2021, 57: 413
doi: 10.11900/0412.1961.2020.00513
[71] 丁 俊, 王章洁. 高熵合金中的局域化学有序 [J]. 金属学报, 2021, 57: 413
[72] Zhang Z R, Armstrong D E J, Grant P S. The effects of irradiation on CrMnFeCoNi high-entropy alloy and its derivatives [J]. Prog. Mater. Sci., 2022, 123: 100807
doi: 10.1016/j.pmatsci.2021.100807
[73] Liu L Q, Liu X J, Du Q, et al. Local chemical ordering and its impact on radiation damage behavior of multi-principal element alloys [J]. J. Mater. Sci. Technol., 2023, 135: 13
doi: 10.1016/j.jmst.2022.05.062
[74] Su Z X, Ding J, Song M, et al. Enhancing the radiation tolerance of high-entropy alloys via solute-promoted chemical heterogeneities [J]. Acta Mater., 2023, 245: 118662
doi: 10.1016/j.actamat.2022.118662
[75] Ullah M W, Aidhy D S, Zhang Y W, et al. Damage accumulation in ion-irradiated Ni-based concentrated solid-solution alloys [J]. Acta Mater., 2016, 109: 17
doi: 10.1016/j.actamat.2016.02.048
[76] Liu L Q. Radiation damage behavior and the underlying mechanism of NiFeCr-based multi-principal element alloys by molecular dynamics simulations [D]. Beijing: University of Science and Technology Beijing, 2024
[76] 刘乐青. NiFeCr系多主元合金辐照损伤行为及其机理的分子动力学研究 [D]. 北京: 北京科技大学, 2024
[77] Tan L Z, Ali K, Ghosh P S, et al. Design principles of low-activation high entropy alloys [J]. J. Alloys Compd., 2022, 907: 164526
doi: 10.1016/j.jallcom.2022.164526
[78] Pu G, Lin L W, Ang R, et al. Outstanding radiation tolerance and mechanical behavior in ultra-fine nanocrystalline Al1.5CoCrFeNi high entropy alloy films under He ion irradiation [J]. Appl. Surf. Sci., 2020, 516: 146129
doi: 10.1016/j.apsusc.2020.146129
[79] Zhao Y F, Chen H H, Zhang D D, et al. Unusual He-ion irradiation strengthening and inverse layer thickness-dependent strain rate sensitivity in transformable high-entropy alloy/metal nanolaminates: A comparison of Fe50Mn30Co10Cr10/Cu vs Fe50Mn30Co10Ni10/Cu [J]. J. Mater. Sci. Technol., 2022, 116: 199
doi: 10.1016/j.jmst.2021.10.036
[80] Du J L, Jiang S H, Cao P P, et al. Superior radiation tolerance via reversible disordering-ordering transition of coherent superlattices [J]. Nat. Mater., 2023, 22: 442
doi: 10.1038/s41563-022-01260-y
[81] Cao P P. Tuning mechanical properties and irradiation resistance of FCC-based multi-principal element alloys via nano-precipitation [D]. Beijing: University of Science and Technology Beijing, 2022
[81] 曹培培. 基于纳米析出调控FCC系多主元合金的力学性能和辐照性能 [D]. 北京: 北京科技大学, 2022
[82] Peng X Y, Cao P P, Liu D, et al. On the origin of superior stability of coherent nanoparticles under ion irradiation [J]. Mater. Des., 2024, 247: 113393
doi: 10.1016/j.matdes.2024.113393
[83] Yang C, Wang B Y, Shen G Y, et al. High-throughput design of a light and strong refractory eutectic medium entropy alloy with outstanding He-ion irradiation resistance [J]. Sci. Adv., 2025, 11: eadq6828
doi: 10.1126/sciadv.adq6828
[1] 郑玉峰, 谌雨农. 纯Mo及钼基可降解金属材料的研究现状与发展趋势[J]. 金属学报, 2026, 62(5): 905-922.
[2] 陈光, 陈奉锐, 朱德民, 李贵忠, 李罗, 宋伟东, 王子特, 相恒高, 陈旸, 祁志祥. 聚片孪生功能基元序构的高性能TiAl合金[J]. 金属学报, 2026, 62(4): 541-549.
[3] 王建峰, 许珍木, 刘战, 高转妮, 占小红. 超声振动对TC4钛合金窄间隙激光焊接组织及强化机理的影响[J]. 金属学报, 2026, 62(3): 406-420.
[4] 蒋志达, 胥杨洋, 于佳新, 刘文才, 朱浩文, 吴国华, 尚郑平. 高温无氧轧制Cu/1060Al/Cu三层复合材料的力学和导电性能[J]. 金属学报, 2026, 62(3): 431-444.
[5] 江国龙, 周霞. 超声辅助下Mg/Mg-Zn-Al钎焊界面行为的分子动力学模拟[J]. 金属学报, 2026, 62(2): 372-382.
[6] 王启勇, 李晓博, 刘小超, 王心成, 张泰瑞, 倪中华, 陈彪. 低碳钢预制涡流搅拌摩擦焊工艺研究[J]. 金属学报, 2026, 62(1): 217-234.
[7] 张天宇, 张鹏, 肖娜, 王小海, 刘国强, 杨志刚, 张弛. 奥氏体化温度对2 GPa超高强钢显微组织和力学性能的影响[J]. 金属学报, 2025, 61(9): 1353-1363.
[8] 王洪瑛, 姚志浩, 李大禹, 郭婧, 姚凯俊, 董建新. 高 γ' 相含量粉末及变形高温合金组织和力学性能的异同性[J]. 金属学报, 2025, 61(9): 1364-1374.
[9] 吴志勇, 邵徽凡, 蔡长春, 曾敏, 王振军, 王艳丽, 陈雷, 熊博文. 斜纹碳布缝合织物结构增强铝基复合材料的高温拉伸及断裂行为[J]. 金属学报, 2025, 61(9): 1387-1402.
[10] 肖文龙, 臧晨阳, 郭锦涛, 冯佳文, 马朝利. 基于原位电阻法的7A65铝合金厚板双级时效工艺[J]. 金属学报, 2025, 61(8): 1153-1164.
[11] 刘继浩, 迟宏宵, 武会宾, 马党参, 周健, 谷金波. 喷射成形工艺对M3高速钢碳化物特征及力学性能的影响[J]. 金属学报, 2025, 61(8): 1229-1244.
[12] 葛蓬华, 张勇, 李志明. 异构FeCoNi中熵合金的软磁与力学行为[J]. 金属学报, 2025, 61(7): 1119-1128.
[13] 韩晓东, 安子冰, 毛圣成, 龙海波, 杨鲁岩, 张泽. 负混合焓合金化推动高强韧合金发展[J]. 金属学报, 2025, 61(7): 953-960.
[14] 谢昂, 陈胜虎, 姜海昌, 戎利建. Nb含量和均质化处理对奥氏体不锈钢铸态组织和力学性能的影响[J]. 金属学报, 2025, 61(7): 1035-1048.
[15] 钦兰云, 张健, 伊俊振, 崔岩峰, 杨光, 王超. 固溶时效对激光沉积修复ZM6合金组织及力学性能的影响[J]. 金属学报, 2025, 61(6): 875-886.