Please wait a minute...
Acta Metall Sin  2019, Vol. 55 Issue (8): 997-1007    DOI: 10.11900/0412.1961.2018.00428
Current Issue | Archive | Adv Search |
Study on the Evolution of Residual Stress During Ageing Treatment in a GH4169 Alloy Disk
Hailong QIN,Ruiyao ZHANG,Zhongnan BI(),Lee Tung Lik,Hongbiao DONG,Jinhui DU,Ji ZHANG
1. Beijing Key Laboratory of Advanced High Temperature Materials, Central Iron and Steel Research Institute, Beijing 100081, China
2. CISRI-GAONA Co. , Ltd. , Beijing 100081, China
3. Department of Engineering, University of Leicester, Leicester, LE1 7RH, UK
4. ISIS Neutron Source, Rutherford Appleton Laboratory, Harwell Oxford, Didcot, OX11 0QX, UK
Cite this article: 

Hailong QIN,Ruiyao ZHANG,Zhongnan BI,Lee Tung Lik,Hongbiao DONG,Jinhui DU,Ji ZHANG. Study on the Evolution of Residual Stress During Ageing Treatment in a GH4169 Alloy Disk. Acta Metall Sin, 2019, 55(8): 997-1007.

Download:  HTML  PDF(13805KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

GH4169 alloy, a precipitation-strengthened nickel-iron base superalloy, has been widely used in aerospace and energy industries due to its excellent high-temperature strength which derived from the coherent phases (γ″ and γ'). To form these precipitates, the manufacturing process of GH4169 usually involves solid solution heat treatment followed by rapid cooling and double ageing heat treatment. Significant residual stresses are induced during rapid cooling and then partially relieved during the subsequent ageing treatment. However, the reduced residual stress after ageing are still large enough to affect the final machining operations, resulting in the component exceeding the dimensional tolerances if they are not well considered. Furthermore, residual stresses in the final components may lead to further distortion beyond estimation during service, which could deteriorate the engine performances. In the present study, the evolution of residual stresses at heating, isothermal ageing, and air-cooling stages of ageing heat treatment in a GH4169 alloy disk was characterized by in situ neutron diffraction. Considering the effect of residual stresses on the precipitation behavior of γ″, two different types of stress-free samples were used as the basis for the stress analysis. The results show that significant residual stresses were induced during water quenching, which were found to be 340.62 MPa tensile in hoop/radial directions and 33.34 MPa compressive in axial direction in the center of the disk. Subsequently, an in situ ageing heat treatment was undertaken at 720 ℃ for 8 h. During the heating stage, the yield strength of the material decreases with increasing temperature, leading to residual stress relaxation through plastic deformation from 340.62 MPa to 227.67 MPa in hoop/radial direction in the disk center. At the isothermal ageing stage, residual stresses relieved apparently by about 40 MPa during the first 100 min, later on a slower linear relaxation remained for the rest of the ageing heat treatment. The strength of the alloy increased and the creep rate decreased due to the formation of γ″ and γ′ strengthening phases, indicating that most of stress relaxation occurred as a result of creep deformation at the early stage of isothermal ageing. The magnitude of residual stress was almost invariable in the subsequent air-cooling stage.

Key words:  superalloy      ageing treatment      residual stress      in situ neutron diffraction     
Received:  07 September 2018     
ZTFLH:  TG115.23  
Fund: Supported by National Key Research and Development Program of China((No.2017YFB0702901));National Natural Science Foundation of China((No.U1708253))

URL: 

https://www.ams.org.cn/EN/10.11900/0412.1961.2018.00428     OR     https://www.ams.org.cn/EN/Y2019/V55/I8/997

Fig.1  In situ neutron diffraction experiment during ageing treatment(a) heating by ceramic blanket under clad insulation (b) covering by heat-preservation cotton
Fig.2  Schematic of neutron path and location for neutron diffraction
Fig.3  Schematic of stress-free s0 sample
Fig.4  Temperature profile of the disk during in situ heating experiment
Fig.5  OM (a) and SEM (b) images of the microstructures of disk after quenching
Fig.6  TEM bright-field images of s0-1 (a, b), s0-2 (c) and s0-5 (d) samples aged for 0.5 h (a, c) and 8 h (b, d)

Temperature

℃

Direction

a / nmStrain / 10-6Stress / MPa
ValueErrorValueErrorValueError

20

Hoop/Radial0.3607680.00000751251.6820.82340.6210.01
Axial0.3598960.0000072-1168.4219.98-33.349.88

340

Hoop/Radial0.3624510.00000851373.1023.48321.859.28
Axial0.3614860.0000079-1292.9821.83-60.709.04

530

Hoop/Radial0.3634920.00000911315.1125.07289.739.33
Axial0.3625500.0000085-1279.6922.59-65.718.99

720

Hoop/Radial0.3644280.00001011165.9927.75227.6710.38
Axial0.3635020.0000088-1351.9624.18-77.749.94
Table 1  Evolution of lattice parameter (a), strain and corresponding residual stress during the heating process
Fig.7  Profiles of a in the center of disk during isothermal ageing process
Fig.8  Evolution of residual stress in the center of disk during isothermal ageing process on the basis of dynamic non-stress standard sample (a) and static non-stress standard sample (b)
Fig.9  Evolution of residual stress in the center of disk during ageing treatment
Fig.10  Neutron diffraction spectra at the beginning (5 min) and the end (480 min) of creep test in longitudinal direction (a), and the separation of overlapped peak (200) (b)
Fig.11  Evolution of stress fitting error with increasing ageing time
Fig.12  Yield strength of as-quenched materials vs temperature
Fig.13  Evolution of microstructure and mechanical properties of GH4169 alloy during isothermal aging treatment(a) volume fraction of γ″ and γ′(b) average diameter of γ″ and γ′(c) yield strength at room temperature(d) creep strain of as-quenched GH4169 alloy at 720 ℃
[1] Reed R C. The Superalloys: Fundamentals and Applications [M]. Cambridge: Cambridge University Press, 2008: 217
[2] Zhuang J Y, Du J H, Deng Q, et al. Wrought Superalloy GH4169 [M]. Beijing: Metallurgical Industry Press, 2006: 1
[2] (庄景云, 杜金辉, 邓 群等. 变形高温合金GH4169 [M]. 北京: 冶金工业出版社, 2006: 1)
[3] Lu X D, Du J H, Deng Q. High temperature structure stability of GH4169 superalloy [J]. Mater. Sci. Eng., 2013, A559: 623
[4] Du J H, Lu X D, Deng Q, et al. High-temperature structure stability and mechanical properties of novel 718 superalloy [J]. Mater. Sci. Eng., 2007, A452-453: 584
[5] Xie X S, Dong J X, Fu S H, et al. Research and development of γ″ and γ′ strengthened Ni-Fe base superalloy GH4169 [J]. Acta Metall. Sin., 2010, 46: 1289
[5] (谢锡善, 董建新, 付书红等. γ″和γ′相强化的Ni-Fe基高温合金GH4169的研究与发展 [J]. 金属学报, 2010, 46: 1289)
[6] Geng L, Na Y S, Park N K. Continuous cooling transformation behavior of Alloy 718 [J]. Mater. Lett., 1997, 30: 401
[7] Dye D, Conlon K T, Reed R C. Characterization and modeling of quenching-induced residual stresses in the nickel-based superalloy IN718 [J]. Metall. Mater. Trans., 2004, 35A: 1703
[8] Rist M A, James J A, Tin S, et al. Residual stresses in a quenched superalloy turbine disc: Measurements and modeling [J]. Metall. Mater. Trans., 2006, 37A: 459
[9] Withers P J, Bhadeshia H K D K. Residual stress Part 2—Nature and origins [J]. Mater. Sci. Technol., 2001, 17: 366
[10] Aba-Perea P E, Pirling T, Preuss M. In-situ residual stress analysis during annealing treatments using neutron diffraction in combination with a novel furnace design [J]. Mater. Des., 2016, 110: 925
[11] Rolph J, Evans A, Paradowska A, et al. Stress relaxation through ageing heat treatment—A comparison between in situ and ex situ neutron diffraction techniques [J]. C. R. Phys., 2012, 13: 307
[12] Xu P G, Tomota Y. Progress in materials characterization technique based on in situ neutron diffraction [J]. Acta Metall. Sin., 2006, 42: 681
[12] (徐平光, 友田阳. 基于原位中子衍射表征技术的进展 [J]. 金属学报, 2006, 42: 681)
[13] Dong P, Wang H, Li J, et al. Residual stress in welded Beryllium ring by neutron diffraction and finite element modeling [J]. At. Energy Sci. Technol., 2015, 49: 2255
[13] (董 平, 王 虹, 李 建等. 铍环焊接残余应力的中子衍射测试与有限元分析 [J]. 原子能科学技术, 2015, 49: 2255)
[14] Collins D M, D' Souza N, Panwisawas C. In-situ neutron diffraction during stress relaxation of a single crystal nickel-base superalloy [J]. Scr. Mater., 2017, 131: 103
[15] Allen A J, Hutchings M T, Windsor C G, et al. Neutron diffraction methods for the study of residual stress fields [J]. Adv. Phys., 1985, 34: 445
[16] Wagner J N, Hofmann M, Wimpory R, et al. Microstructure and temperature dependence of intergranular strains on diffractometric macroscopic residual stress analysis [J]. Mater. Sci. Eng., 2014, A618: 271
[17] Eto T, Sato A, Mori T. Stress-oriented precipitation of G. P. Zones and θ' in an Al-Cu alloy [J]. Acta Metall., 1978, 26: 499
[18] Li D Y, Chen L Q. Computer simulation of stress-oriented nucleation and growth of θ′ precipitates in Al-Cu alloys [J]. Acta Mater., 1998, 46: 2573
[19] Cheng K Y, Jo C Y, Jin T, et al. Influence of applied stress on the γ′ directional coarsening in a single crystal superalloy [J]. Mater. Des., 2010, 31: 968
[20] Gao M, Harlow D G, Wei R P, et al. Preferential coarsening of γ″ precipitates in Inconel 718 during creep [J]. Metall. Mater. Trans., 1996, 27A: 3391
[21] Qin H L, Bi Z N, Yu H Y, et al. Influence of stress on γ″ precipitation behavior in Inconel 718 during aging [J]. J. Alloys Compd., 2018, 740: 997
[22] Qin H L, Bi Z N, Yu H Y, et al. Assessment of the stress-oriented precipitation hardening designed by interior residual stress during ageing in IN718 superalloy [J]. Mater. Sci. Eng., 2018, A728: 183
[23] Santisteban J R, Daymond M R, James J A, et al. ENGIN-X: A third-generation neutron strain scanner [J]. J. Appl. Cryst., 2006, 39: 812
[24] Pawley G S. Unit-cell refinement from powder diffraction scans [J]. J. Appl. Crystallogr., 1981, 14: 357
[25] Denis S, Sj?str?m S, Simon A. Coupled temperature, stress, phase transformation calculation [J]. Metall. Trans., 1987, 18A: 1203
[26] Aba-Perea P E, Pirlinga T, Withers P J, et al. Determination of the high temperature elastic properties and diffraction elastic constants of Ni-base superalloys [J]. Mater. Des., 2016, 89: 856
[27] Oradei-Basile A, Radavich J F. A current TTT diagram for wrought alloy 718 [A]. Superalloys 718, 625 and Various Derivatives [C]. Pittsburgh: Springer, 1991: 325
[28] Wang Y Z, Dong J X, Zhang M C, et al. Stress relaxation behavior and mechanism of AEREX 350 and Waspaloy superalloys [J]. Mater. Sci. Eng., 2016, A678: 10
[29] Hong S J, Chen W P, Wang T W. A diffraction study of the γ″ phase in INCONEL 718 superalloy [J]. Metall. Mater. Trans., 2001, 32A: 1887
[30] Kulawik K, Buffat P A, Kruk A, et al. Imaging and characterization of γ′ and γ″ nanoparticles in Inconel 718 by EDX elemental mapping and FIB—SEM tomography [J]. Mater. Charact., 2015, 100: 74
[31] Liu Y, Qin S W, Zuo X W, et al. Finite element simulation and experimental verification of quenching stress in fully through-hardened cylinders [J]. Acta Metall. Sin., 2017, 53: 733
[31] (刘 玉, 秦盛伟, 左训伟等. 全淬透圆柱件淬火应力的有限元模拟及实验验证 [J]. 金属学报, 2017, 53: 733)
[32] Foss B J, Gray S, Hardy M C, et al. Analysis of shot-peening and residual stress relaxation in the nickel-based superalloy RR1000 [J]. Acta Mater., 2013, 61: 2548
[33] Zhang F, Cao W S, Zhang C, et al. Simulation of co-precipitation kinetics of γ′ and γ″ in superalloy 718 [A]. Proceedings of the 9th International Symposium on Superalloy 718 & Derivatives: Energy, Aerospace, and Industrial Applications [C]. Pittsburgh: Springer, 2018: 147
[34] Fisk M, Ion J C, Lindgren L E. Flow stress model for IN718 accounting for evolution of strengthening precipitates during thermal treatment [J]. Comput. Mater. Sci., 2104, 82: 531
[35] Oblak J M, Paulonis D F, Duvall D S. Coherency strengthening in Ni base alloys hardened by D022γ′ precipitates [J]. Metall. Trans., 1974, 5: 143
[36] Han Y F, Chaturvedi M C. A study of back stress during creep deformation of a superalloy inconel 718 [J]. Mater. Sci. Eng., 1987, 85: 59
[37] Chaturvedi M C, Han Y F. Effect of particle size on the creep rate of superalloy Inconel 718 [J]. Mater. Sci. Eng., 1987, 89: L7
[38] Kuo C M, Yang Y T, Bor H Y, et al. Aging effects on the microstructure and creep behavior of Inconel 718 superalloy [J]. Mater. Sci. Eng., 2009, A510-511: 289
[1] BI Zhongnan, QIN Hailong, LIU Pei, SHI Songyi, XIE Jinli, ZHANG Ji. Research Progress Regarding Quantitative Characterization and Control Technology of Residual Stress in Superalloy Forgings[J]. 金属学报, 2023, 59(9): 1144-1158.
[2] ZHENG Liang, ZHANG Qiang, LI Zhou, ZHANG Guoqing. Effects of Oxygen Increasing/Decreasing Processes on Surface Characteristics of Superalloy Powders and Properties of Their Bulk Alloy Counterparts: Powders Storage and Degassing[J]. 金属学报, 2023, 59(9): 1265-1278.
[3] BAI Jiaming, LIU Jiantao, JIA Jian, ZHANG Yiwen. Creep Properties and Solute Atomic Segregation of High-W and High-Ta Type Powder Metallurgy Superalloy[J]. 金属学报, 2023, 59(9): 1230-1242.
[4] MA Dexin, ZHAO Yunxing, XU Weitai, WANG Fu. Effect of Gravity on Directionally Solidified Structure of Superalloys[J]. 金属学报, 2023, 59(9): 1279-1290.
[5] CHEN Jia, GUO Min, YANG Min, LIU Lin, ZHANG Jun. Effects of W Concentration on Creep Microstructure and Property of Novel Co-Based Superalloys[J]. 金属学报, 2023, 59(9): 1209-1220.
[6] JIANG He, NAI Qiliang, XU Chao, ZHAO Xiao, YAO Zhihao, DONG Jianxin. Sensitive Temperature and Reason of Rapid Fatigue Crack Propagation in Nickel-Based Superalloy[J]. 金属学报, 2023, 59(9): 1190-1200.
[7] GONG Shengkai, LIU Yuan, GENG Lilun, RU Yi, ZHAO Wenyue, PEI Yanling, LI Shusuo. Advances in the Regulation and Interfacial Behavior of Coatings/Superalloys[J]. 金属学报, 2023, 59(9): 1097-1108.
[8] ZHAO Peng, XIE Guang, DUAN Huichao, ZHANG Jian, DU Kui. Recrystallization During Thermo-Mechanical Fatigue of Two High-Generation Ni-Based Single Crystal Superalloys[J]. 金属学报, 2023, 59(9): 1221-1229.
[9] FENG Qiang, LU Song, LI Wendao, ZHANG Xiaorui, LI Longfei, ZOU Min, ZHUANG Xiaoli. Recent Progress in Alloy Design and Creep Mechanism of γ'-Strengthened Co-Based Superalloys[J]. 金属学报, 2023, 59(9): 1125-1143.
[10] DU Jinhui, BI Zhongnan, QU Jinglong. Recent Development of Triple Melt GH4169 Alloy[J]. 金属学报, 2023, 59(9): 1159-1172.
[11] LI Jiarong, DONG Jianmin, HAN Mei, LIU Shizhong. Effects of Sand Blasting on Surface Integrity and High Cycle Fatigue Properties of DD6 Single Crystal Superalloy[J]. 金属学报, 2023, 59(9): 1201-1208.
[12] WANG Lei, LIU Mengya, LIU Yang, SONG Xiu, MENG Fanqiang. Research Progress on Surface Impact Strengthening Mechanisms and Application of Nickel-Based Superalloys[J]. 金属学报, 2023, 59(9): 1173-1189.
[13] LU Nannan, GUO Yimo, YANG Shulin, LIANG Jingjing, ZHOU Yizhou, SUN Xiaofeng, LI Jinguo. Formation Mechanisms of Hot Cracks in Laser Additive Repairing Single Crystal Superalloys[J]. 金属学报, 2023, 59(9): 1243-1252.
[14] ZHANG Jian, WANG Li, XIE Guang, WANG Dong, SHEN Jian, LU Yuzhang, HUANG Yaqi, LI Yawei. Recent Progress in Research and Development of Nickel-Based Single Crystal Superalloys[J]. 金属学报, 2023, 59(9): 1109-1124.
[15] LIU Xingjun, WEI Zhenbang, LU Yong, HAN Jiajia, SHI Rongpei, WANG Cuiping. Progress on the Diffusion Kinetics of Novel Co-based and Nb-Si-based Superalloys[J]. 金属学报, 2023, 59(8): 969-985.