School of Materials Science and Engineering, South China University of Technology, Guangzhou 510640, China
Cite this article:
Liheng LIU,Chunshan CHE,Gang KONG,Jintang LU,Shuanghong ZHANG. DESTABILIZATION MECHANISM OF Fe-Al INHIBITION LAYER IN Zn-0.2%Al HOT-DIP GALVANIZING COATING AND RELATED THERMODYNAMIC EVALUATION. Acta Metall Sin, 2016, 52(5): 614-624.
The formation of a uniform Fe-Al inhibition layer with a proper thickness at steel interface during continuous hot-dip galvanizing process is a crucial issue for industrial production. The inhibition layer prohibits the nucleation and growth of brittle Fe-Zn intermetallic compounds which deteriorate the adhesion of the galvanizing coating and result in an inhomogeneous distribution of the coating. The inhibition layer was identified to be Fe2Al5 with some Zn dissolved in it. But Fe2Al5 inhibition layer was damaged with galvanized time increasing, will lose the inhibition to the Fe-Zn reaction. Nevertheless, there is no systematic and comprehensive investigation the causes of the inhibition layer is damaged. The aim of this work is to clarify the destabilization mechanism of Fe2Al5 inhibition layer. In the present study, the mass fraction of 0.2%Al was added into the zinc bath at 450 ℃ for hot-dip galvanizing. SEM was used to observe the structure characteristics of the hot-dip galvanized coating. EDS was used to quantitatively analyze the micro area components of phases and also used its line scan and mapping scan to qualitatively analyze the element change of the coating cross section. By means of the Miedema model and the Toop model, the thermodynamic values of the binary Fe-Al, Fe-Zn and ternary Fe2Al5Znx (η) intermetallic compounds (IMC) in the coatings were calculated. The fundamental reason for the Fe-Zn reaction caused by Fe2Al5 destabilization with galvanized time increasing was analyzed. The results show that because Fe-Al IMC which is generate preferentially had more stable thermodynamic property than Fe-Zn IMC, the continuous Fe2Al5 intermetallic compound inhibition layer was produced preferentially at steel and zinc bath interface which inhibit the Fe-Zn reaction. However, with the galvanized time increasing, Fe2Al5 destabilization which led to the loss of inhibitory effect of Fe-Zn reaction and produced FeZn10 (δ) . There are two kinds of destabilization mechanism of Fe2Al5 inhibition layer, one is that the local depletion of Al at Fe2Al5 and zinc bath interface result in erosion of Fe2Al5 by Zn and the formed Fe2Al5Znx caused the decrease of the systematic thermodynamic stability which led to erosion and decomposition of Fe2Al5 by Zn. At the same time, FeZn10 (δ) phase was produced between the Fe2Al5 and zinc bath interface. The phase transformation process can be described as: Fe2Al5→η→L+η→L+η+δ→L+δ. The other kind of destabilization mechanism is Zn diffused to the steel substrate by Fe2Al5 grain boundaries and directly produced δ phase between Fe2Al5 and steel substrate interface, which caused outburst of Fe2Al5. The two kinds of Fe2Al5 destabilization mechanism are mutual coexistence and mutual competition, in particular conditions may be a mechanism to occupy absolute advantage.
Fund: Supported by International Lead and Zinc Research Organization Funded Projects (No.ILZRO/IZA/CN201212), Project on the Integration of Industry, Education and Research of Guangdong Province (No.2012B091100312) and Fundamental Research Funds for the Central Universities of China (No.2012ZM0011)
Fig.1 Cross-sectional SEM images of coating after hot-dip galvanizing at 450 ℃ for 10 s (a), 30 s (b), 90 s (c), 300 s (d) and corresponding EDS line scan diagrams of bold arrows in Figs.a~d (a1~d1)
Micro square
Atomic fraction / %
Phase
Al
Fe
Zn
1
-
1.96
98.04
L
2
20.74
63.62
15.64
Rich-Al phase
3
50.24
22.98
26.78
η+δ
4
1.74
7.34
90.92
δ
5
8.21
6.93
84.86
δ
6
2.09
12.22
85.69
δ
7
57.33
20.79
21.88
η+δ
8
3.25
9.23
87.52
δ
9
4.74
7.79
87.47
δ
Table 1 EDS analysis results for micro squares 1~9 in Fig.1
Fig.2 SEM image of rectangular region in Fig.1b (a), and EDS mapping scan analyses of Al (b), Fe (c) and Zn (d)
Fig.3 Fe-Al-Zn isothermal section of the Zn corner at 450 ℃ (after <30 min of galvanizing)[32]
Element
V
?*
nWS
W/P
Fe
7.09
4.93
5.55
1.0
Al
10.00
4.20
2.70
1.9
Zn
9.17
4.10
2.30
1.4
Table 2 Property parameters of Fe, Al and Zn elements[25]
IMC
ΔHAB / (kJmol-1)
GABE / (kJmol-1)
aFe
aAl or Zn
ΔGθ / (kJmol-1)
Fe2Al5
-21.85
-19.28
6.03×10-6
0.595
-22.87
FeAl3
-19.18
-16.93
4.08×10-6
0.693
-20.31
Γ (Fe3Zn10)
-2.87
-2.46
4.07×10-2
0.760
-5.71
Γ1 (Fe5Zn21)
-2.68
-2.29
3.22×10-2
0.770
-5.24
δ (FeZn10)
-1.12
-0.96
1.67×10-2
0.903
-2.79
ζ (FeZn13)
-0.89
-0.76
1.32×10-2
0.923
-2.31
Table 3 Thermodynamic values of Fe-Al and Fe-Zn intermetallic compounds (IMC)
Fig.4 Schematic of Fe2Al5 crystal structure (a) and projection in the a axis direction (b)
Fig.5 Schematics of coating layer formation in a Zn-0.20%Al galvanizing at 450 ℃
[1]
Marder A R.Prog Mater Sci, 2000; 45: 191
[2]
Shao D W, He Z R, Zhang Y H, He Y.Hot Working Technol, 2012; 41: 122
[2]
(邵大伟, 贺志荣, 张永宏, 何应. 热加工工艺, 2012; 41: 122)
[3]
Dionne S.JOM-US, 2006; 58(3): 32
[4]
Wang Y, Xing J D, Ma S Q, Liu G Z, Fu H G, Jia S.J Mater Eng Perform, 2015; 24: 2444
[5]
Kim Y, Shin K S, Jeon S H, Chin K G, Lee J.Corros Sci, 2014; 85: 364
Inagaki J, Sakurai M, Watanabe T.Tetsu Hagané, 1993; 79: 1273
[21]
(稲垣淳一, 櫻井理孝, 渡辺豊文.铁と钢, 1993; 79: 1273)
[22]
Kato T, Nunome K, Kaneko K, Saka H. Acta Mater, 2000; 48: 2257
[23]
Sun W X, Yan D R, Chen X G, Dong Y C, Li X Z.Acta Phys Sin, 2010; 59: 2228
[23]
(孙文秀, 阎殿然, 陈学广, 董艳春, 李香芝. 物理学报, 2010; 59: 2228)
[24]
Kato C, Koumura H, Mochizuki K, Morito N. US Pat,80106, 1995
[25]
Miedema A R, Niessen A K, Deboer F R, Boom R, Matten W C.Cohesion in Metals: Transition Metal Alloys. Amsterdam: North-Holland Publishing Co., 1989: 38
[26]
Zhang R F, Rajan K.Chem Phys Lett, 2014; 612: 177
[27]
Ding X Y, Fan P, Han Q Y.Acta Metall Sin, 1994; 30: 49