High-Throughput Preparation and Corrosion Resistance of Yb-Gd Modified Si Bond Coat
WANG Yehan1,2, LV Xirui2, SHI Jinyu1,2, LEI Yiming2, ZHANG Jie2(), WANG Jingyang2
1 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
2 Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
引用本文:

王晔晗, 吕熙睿, 石金瑜, 雷一明, 张洁, 王京阳. Yb-Gd改性硅黏结层的高通量制备与耐腐蚀性能[J]. 金属学报, 2026, 62(10): 1676-1686.
Yehan WANG, Xirui LV, Jinyu SHI, Yiming LEI, Jie ZHANG, Jingyang WANG. High-Throughput Preparation and Corrosion Resistance of Yb-Gd Modified Si Bond Coat[J]. Acta Metall Sin, 2026, 62(10): 1676-1686.

全文: PDF(3043 KB)   HTML
摘要: 

新一代高推重比航空发动机对环境障涂层的服役寿命和温度提出更高要求,向硅黏结层中掺杂稀土元素有望提升其耐高温和耐腐蚀性能,而成分变化是稀土改性硅黏结层材料相组成及性能变化的根本原因。本工作通过多靶磁控溅射共沉积等方法,高通量制备、表征了Yb-Gd稀土改性硅黏结层材料芯片,研究了Yb-Gd硅化物的不同成分组合在1100、1300 ℃空气气氛和1300 ℃水蒸气-空气气氛下的相组成及微观形貌变化。结果表明,Yb-Gd-Si三元稀土硅化物高温氧化后的主要产物为RE9.33(SiO4)6O2和RE2SiO5 (RE = Gd、Yb),随着氧化温度的升高,RE2SiO5由X1相转变为X2相。Yb-Gd-Si三元稀土硅化物高温水氧腐蚀后的形貌随成分变化而存在差异,其腐蚀机制为优先发生氧化,随后在水蒸气气流作用下,Si和RE以Si(OH)4和RE(OH)3的形式耗散,且在不同Si含量的影响下,产生不同形貌。

关键词 : 黏结层,  稀土硅化物,  高通量方法,  组合材料芯片,  物理气相沉积,  磁控溅射    
Abstract:

Silicon carbide fiber-reinforced silicon carbide ceramic matrix composites (SiCf/SiC CMCs) are considered strategic thermal, structural materials for advanced aircraft engines due to their lightweight, high specific strength, and excellent high-temperature capability. In harsh combustion environments, environmental barrier coatings (EBCs) are required to protect SiCf/SiC CMC from water vapor corrosion and low-melting-point oxide corrosion, ensuring the long-term serviceability of SiCf/SiC components. The development of next-generation high thrust-to-weight ratio aero engines has imposed more stringent requirements on the service life and temperature resistance of EBCs. Typical EBCs consist of a ceramic topcoat and a Si bond coat. However, the water vapor corrosion and oxidation of Si are essential factors contributing to EBC failure during service. Doping rare earth (RE) elements into the Si bond coat is expected to enhance its high-temperature capability and corrosion resistance, making it a promising strategy for developing advanced bond coat materials. For rare earth element-modified Si bond coat materials, composition variations fundamentally influence performance changes, including phase composition. However, the composition-property relationship of rare earth-modified Si bond coats remains unclear. In this study, Yb-Gd modified Si bond coat material chips were prepared using multi-target magnetron sputtering for co-deposition and were characterized using a high-throughput method. Transformation trends were identified by analyzing the phase composition and micromorphological changes in different Yb-Gd silicide compositions under extreme conditions (1100 and 1300 oC in an air atmosphere and 1300 oC in a water vapor-air atmosphere). It was found that the primary oxidation products of the Yb-Gd-Si ternary rare earth silicide at high temperatures are RE9.33(SiO4)6O2 and RE2SiO5 (where RE = Gd, Yb). RE2SiO5 undergoes a phase transformation from X1 to X2 as oxidation temperature increases. The morphology of Yb-Gd-Si silicide varies with composition after high-temperature water vapor corrosion. The corrosion mechanism involves initial oxidation, followed by the dissipation of Si and RE in the form of Si(OH)4 and RE(OH)3 under water vapor flow, where different silicon contents lead to distinct corrosion morphologies.

Key words: bond coat    rare earth silicide    high-throughput method    combination material chip    physical vapor deposition    magnetron sputtering
收稿日期: 2025-01-03     
ZTFLH:  TG174.4  
基金资助:国家重点研发计划项目(2022YFB3707700);国家自然科学基金项目(U21A2063);国家自然科学基金项目(52372071);国家自然科学基金项目(52302076);中国科学院国际伙伴计划项目(172GJHZ2022094FN);中国航发集团产学研合作项目(HFZL2023CXY022);兴辽英才计划项目(XLYC2002018);兴辽英才计划项目(XLYC2203090)
通讯作者: 张 洁,jiezhang@imr.ac.cn,主要从事极端环境陶瓷涂层应用基础研究
Corresponding author: ZHANG Jie, professor, Tel: (024)23970490, E-mail: jiezhang@imr.ac.cn
作者简介: 王晔晗,男,1999年生,硕士
图1  组合材料芯片制备过程示意图和制备态Yb-Gd-Si组合材料芯片光学照片
图2  组合材料芯片元素成分分布图以及根据成分得到的三元组分图
图3  不同Gd / Yb (原子比,下同)样品及Gd / Si样品(RE / Si = 0.6)的微区XRD谱
图4  组合材料芯片在1100和1300 ℃空气氧化后不同Gd / Yb成分点的微区XRD谱
图5  特征点在组合材料芯片上的位置、1300 ℃空气氧化后微区XRD谱以及表面和截面SEM像
PointStatePositionAtomic fraction of element / %RE / SiGd / Yb
SiGdYbO
L4As-prepared52.0 ± 0.832.6 ± 2.315.5 ± 1.50.922.10
Air oxidationTop layer14.3 ± 0.617.8 ± 0.78.6 ± 0.859.4 ± 0.81.852.07
Middle layer11.5 ± 0.417.4 ± 0.57.0 ± 0.364.1 ± 0.92.112.49
Bottom layer10.6 ± 0.716.9 ± 0.77.0 ± 0.265.5 ± 1.12.252.44
Steam corrosionTop layer11.9 ± 1.516.7 ± 1.46.4 ± 0.565.1 ± 2.61.952.62
Middle layer10.2 ± 1.116.7 ± 1.46.3 ± 0.766.7 ± 3.02.252.64
Bottom layer7.2 ± 1.914.1 ± 3.15.8 ± 1.072.9 ± 0.32.782.44
F6As-prepared62.5 ± 0.622.2 ± 0.315.3 ± 0.30.601.45
Air oxidationTop layer14.5 ± 1.116.7 ± 0.59.1 ± 0.659.7 ± 2.21.781.85
Middle layer12.3 ± 0.616.5 ± 0.68.8 ± 0.462.5 ± 1.42.041.88
Bottom layer9.8 ± 1.414.6 ± 0.97.9 ± 0.467.7 ± 2.52.291.85
Steam corrosionTop layer10.7 ± 0.312.2 ± 0.36.5 ± 0.270.5 ± 0.41.761.87
Middle layer10.1 ± 0.913.3 ± 0.96.8 ± 0.469.8 ± 2.11.981.97
Bottom layer7.6 ± 1.213.2 ± 1.46.4 ± 0.572.8 ± 2.72.562.06
A2As-prepared73.3 ± 5.013.9 ± 5.212.7 ± 0.30.361.10
Air oxidationTop layer17.3 ± 0.913.1 ± 0.98.3 ± 0.461.4 ± 1.31.231.58
Middle layer12.3 ± 0.913.3 ± 0.78.5 ± 0.165.9 ± 0.51.781.57
Bottom layer10.5 ± 1.110.6 ± 1.77.3 ± 1.071.5 ± 0.41.701.45
Steam corrosionTop layer16.8 ± 2.012.0 ± 1.27.8 ± 0.463.5 ± 1.31.181.54
Middle layer11.0 ± 1.313.0 ± 1.17.8 ± 0.268.2 ± 0.91.911.67
Bottom layer10.4 ± 0.510.2 ± 0.76.7 ± 0.572.7 ± 1.41.621.52
表1  组合材料芯片在1300 ℃空气和水蒸气氧化1 h后特征点截面不同位置EDS半定量成分分析
图6  组合材料芯片在1300 ℃水氧腐蚀1 h后不同Gd / Yb成分点的微区XRD谱
图7  1300 ℃水氧腐蚀后,芯片氧化膜生长率随成分的变化、微区XRD谱以及表面和截面的SEM像
[1] Padture N P. Advanced structural ceramics in aerospace propulsion[J]. Nat. Mater., 2016, 15: 804
doi: 10.1038/nmat4687 pmid: 27443899
[2] Menon M N, Fang H T, Wu D C, et al. Creep and stress rupture behavior of an advanced silicon nitride: Part I, experimental observations[J]. J. Am. Ceram. Soc., 1994, 77: 1217
doi: 10.1111/jace.1994.77.issue-5
[3] Liu Q M, Huang S Z, Liu J, et al. Progress and application of high temperature structural materials on aero-engine[J]. Gas Turbine Exp. Res., 2014, 27(4): 51
[3] 刘巧沐, 黄顺洲, 刘 佳 等. 高温材料研究进展及其在航空发动机上的应用[J]. 燃气涡轮试验与研究, 2014, 27(4): 51
[4] Li L B. Research progress on application and airworthiness compliance validation of ceramicmatrix composites in aeroengines[J]. Acta Mater. Compos. Sin., 2025, 42(1): 54
[4] 李龙彪. 陶瓷基复合材料在航空发动机应用与适航符合性验证研究进展[J]. 复合材料学报, 2025, 42(1): 54
[5] Poerschke D L, Jackson R W, Levi C G. Silicate deposit degradation of engineered coatings in gas turbines: Progress toward models and materials solutions[J]. Annu. Rev. Mater. Res., 2017, 47: 297
doi: 10.1146/matsci.2017.47.issue-1
[6] Eaton H E, Linsey G D. Accelerated oxidation of SiC CMC's by water vapor and protection via environmental barrier coating approach[J]. J. Eur. Ceram. Soc., 2002, 22: 2741
doi: 10.1016/S0955-2219(02)00141-3
[7] Tejero-Martin D, Bennett C, Hussain T. A review on environmental barrier coatings: History, current state of the art and future developments[J]. J. Eur. Ceram. Soc., 2021, 41: 1747
doi: 10.1016/j.jeurceramsoc.2020.10.057
[8] Wang J Y, Sun L C, Luo Y X, et al. Rare earth silicate environmental barrier coating material: High-entropy design and resistance to CMAS corrosion[J]. Acta Metall. Sin., 2023, 59: 523
doi: 10.11900/0412.1961.2022.00556
[8] 王京阳, 孙鲁超, 罗颐秀 等. 以抗CMAS腐蚀为目标的稀土硅酸盐环境障涂层高熵化设计与性能提升[J]. 金属学报, 2023, 59: 523
doi: 10.11900/0412.1961.2022.00556
[9] Wang H Y, Luo Z X, Sun L C, et al. Comprehensive microstructural characterization and CMAS infiltration resistance of ytterbium disilicate coatings with lamellar and quasi-columnar structures[J]. Corros. Sci., 2023, 221: 111316
doi: 10.1016/j.corsci.2023.111316
[10] Harder B J. Oxidation performance of Si-HfO2 environmental barrier coating bond coats deposited via plasma spray-physical vapor deposition[J]. Surf. Coat. Technol., 2020, 384: 125311
doi: 10.1016/j.surfcoat.2019.125311
[11] Morigayama H, Miyazaki T, Usami S, et al. Phase stability of Yb-Gd-Si ternary alloys at elevated temperature[J]. J. Alloys Compd., 2020, 825: 154098
doi: 10.1016/j.jallcom.2020.154098
[12] Golden R A, Opila E J. High-temperature oxidation of yttrium silicides[J]. J. Mater. Sci., 2018, 53: 3981
doi: 10.1007/s10853-017-1823-x
[13] Okamoto H. Gd-Si (gadolinium-silicon)[J]. J. Phase Equilib. Diffus., 2009, 30: 213
doi: 10.1007/s11669-009-9477-2
[14] Kim J, Jung I H. Critical evaluation and thermodynamic optimisation of the Si-RE systems: Part II. Si-RE system (RE = Gd, Tb, Dy, Ho, Er, Tm, Lu and Y)[J]. J. Chem. Thermodyn., 2015, 81: 273
doi: 10.1016/j.jct.2014.08.014
[15] Miyazaki T, Usami S, Arai Y, et al. Oxidation behavior of ytterbium silicide in air and steam[J]. Intermetallics, 2021, 128: 106992
doi: 10.1016/j.intermet.2020.106992
[16] Zhu D M, Farmer S, McCue T R, et al. Environmental stability and oxidation behavior of HfO2-Si and YbGd(O) based environmental barrier coating systems for SiC/SiC ceramic matrix composites[R]. Cleveland: National Aeronautics and Space Administration, 2017
[17] Zhu D M. Development and property evaluation of selected HfO2-silicon and rare earth-silicon based bond coats and environmental barrier coating systems for SiC/SiC ceramic matrix composites[R]. Cleveland: National Aeronautics and Space Administration, 2016
[18] Zhu D M. Advanced environmental barrier coatings for SiC/SiC ceramic matrix composite turbine components[A]. Engineered Ceramics: Current Status and Future Prospects[M]. Hoboken: Wiley, 2016: 187
[19] Xiang H M, Xing Y, Dai F Z, et al. High-entropy ceramics: Present status, challenges, and a look forward[J]. J. Adv. Ceram., 2021, 10: 385
doi: 10.1007/s40145-021-0477-y
[20] Rajan K. Combinatorial materials sciences: experimental strategies for accelerated knowledge discovery[J]. Annu. Rev. Mater. Res., 2008, 38: 299
doi: 10.1146/matsci.2008.38.issue-1
[21] Lv X R, Lei Y M, Zhang Z, et al. Accelerating the design of multicomponent rare earth silicates for SiCf/SiC CMC by combinatorial material chip design and high throughput screening[J]. J. Mater. Sci. Technol., 2023, 150: 96
doi: 10.1016/j.jmst.2022.11.043
[22] Miracle D B, Li M, Zhang Z H, et al. Emerging capabilities for the high-throughput characterization of structural materials[J]. Annu. Rev. Mater. Res., 2021, 51: 131
doi: 10.1146/annurev-matsci-080619-022100
[23] Harris L A, Finch C B. Crystallographic data for Er2SiO5 and Y2SiO5 [J]. Am. Mineral., 1965, 50: 1493
[24] Hu W P, Zhang J, Nian H Q, et al. Phase evolution of reactive sputtering synthesized holmium silicate coatings[J]. J. Am. Ceram. Soc., 2019, 102: 490
doi: 10.1111/jace.2019.102.issue-1
[25] Alves M F R P, Santos C, Olhero S M, et al. Pressureless sintered lithium disilicate glass-ceramics: Influence of particle size and crystallization state[J]. J. Eur. Ceram. Soc., 2024, 44: 6135
doi: 10.1016/j.jeurceramsoc.2024.03.012
[26] Takeda O, Uda T, Okabe T H. Treatise on Process Metallurgy[M]. Amsterdam: Elsevier, 2014: 995
[27] Zhong X, Liang R H, Hong D, et al. Corrosion behavior and mechanism of ytterbium silicates environmental barrier coatings subjected to thermal cycling in water vapor[J]. J. Am. Ceram. Soc., 2024, 107: 387
doi: 10.1111/jace.v107.1
[28] Wang Y W, Niu Y R, Zhong X, et al. Water vapor corrosion behaviors of plasma sprayed RE2SiO5 (RE = Gd, Y, Er) coatings[J]. Corros. Sci., 2020, 167: 108529
doi: 10.1016/j.corsci.2020.108529
[1] 张建东, 席晓翀, 凌永生, 曾繁荣, 单卿, 贾文宝. (AlCrTaTiZr)N x 阻氚涂层制备及其表面氢同位素吸附[J]. 金属学报, 2025, 61(12): 1781-1789.
[2] 李聪, 王猛, 屠汉俊, 施立群. Y掺杂Ti膜的吸放氢行为[J]. 金属学报, 2024, 60(6): 826-836.
[3] 王郑, 王振玉, 汪爱英, 杨巍, 柯培玲. 微弧氧化时间对锆合金表面MAO/Cr复合涂层结构与性能的影响[J]. 金属学报, 2024, 60(5): 691-698.
[4] 刘畅, 吴戈, 吕坚. 纳米结构多主元合金的力学行为及强塑化机制[J]. 金属学报, 2024, 60(1): 16-29.
[5] 黄鼎, 乔岩欣, 杨兰兰, 王金龙, 陈明辉, 朱圣龙, 王福会. 基体表面喷丸处理对纳米晶涂层循环氧化行为的影响[J]. 金属学报, 2023, 59(5): 668-678.
[6] 曹庆平, 吕林波, 王晓东, 蒋建中. 物理气相沉积制备金属玻璃薄膜及其力学性能的样品尺寸效应[J]. 金属学报, 2021, 57(4): 473-490.
[7] 吴玉程, 高志强, 徐光青, 刘家琴, 轩海成, 刘友好, 衣晓飞, 陈静武, 韩培德. 烧结NdFeB永磁材料腐蚀与防护的研究现状及挑战[J]. 金属学报, 2021, 57(2): 171-181.
[8] 刘艳梅, 王铁钢, 郭玉垚, 柯培玲, 蒙德强, 张纪福. Ti-B-N纳米复合涂层的设计、制备及性能[J]. 金属学报, 2020, 56(11): 1521-1529.
[9] 李文涛,王振玉,张栋,潘建国,柯培玲,汪爱英. 电弧复合磁控溅射结合热退火制备Ti2AlC涂层[J]. 金属学报, 2019, 55(5): 647-656.
[10] 杨莎莎,杨峰,陈明辉,牛云松,朱圣龙,王福会. N掺杂对磁控溅射Ta涂层微观结构与耐磨损性能的影响[J]. 金属学报, 2019, 55(3): 308-316.
[11] 吴厚朴,田修波,张新宇,巩春志. 双脉冲HiPIMS放电特性及CrN薄膜高速率沉积[J]. 金属学报, 2019, 55(3): 299-307.
[12] 时惠英, 杨超, 蒋百灵, 黄蓓, 王迪. 双脉冲磁控溅射峰值靶电流密度对TiN薄膜结构与力学性能的影响[J]. 金属学报, 2018, 54(6): 927-934.
[13] 隋旭东,李国建,王强,秦学思,周向葵,王凯,左立建. 钛合金切削用Ti1-xAlxN涂层的制备及其切削性能研究*[J]. 金属学报, 2016, 52(6): 741-746.
[14] 楼白杨,王宇星. Mo含量对CrMoAlN薄膜微观结构和摩擦磨损性能的影响*[J]. 金属学报, 2016, 52(6): 727-733.
[15] 吴法宇,李建伟,齐羿,丁梧桐,樊子铭,周艳文. 粉末靶射频磁控溅射非晶Al2O3薄膜的制备与性能研究*[J]. 金属学报, 2016, 52(12): 1595-1600.