Please wait a minute...
金属学报  2023, Vol. 59 Issue (11): 1475-1486    DOI: 10.11900/0412.1961.2022.00204
  本期目录 | 过刊浏览 |
600℃ NaCl盐雾环境下GH4169合金的腐蚀行为
张伟东1, 崔宇2(), 刘莉1(), 王文泉1, 刘叡1, 李蕊1, 王福会1
1.东北大学 沈阳材料科学国家研究中心东北大学联合研究分部 沈阳 110819
2.中国科学院金属研究所 师昌绪先进材料创新中心 沈阳 110016
Corrosion Behavior of GH4169 Alloy in NaCl Solution Spray Environment at 600oC
ZHANG Weidong1, CUI Yu2(), LIU Li1(), WANG Wenquan1, LIU Rui1, LI Rui1, WANG Fuhui1
1.Shenyang National Laboratory for Materials Science, Northeastern University, Shenyang 110819, China
2.Shi-changxu Innovation Center for Advanced Materials, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
引用本文:

张伟东, 崔宇, 刘莉, 王文泉, 刘叡, 李蕊, 王福会. 600℃ NaCl盐雾环境下GH4169合金的腐蚀行为[J]. 金属学报, 2023, 59(11): 1475-1486.
Weidong ZHANG, Yu CUI, Li LIU, Wenquan WANG, Rui LIU, Rui LI, Fuhui WANG. Corrosion Behavior of GH4169 Alloy in NaCl Solution Spray Environment at 600oC[J]. Acta Metall Sin, 2023, 59(11): 1475-1486.

全文: PDF(5135 KB)   HTML
摘要: 

利用氧化动力学测试,结合微观表征技术,从腐蚀动力学、腐蚀层相组成和组织结构等方面,研究了GH4169合金在600℃的NaCl盐雾环境中的腐蚀行为。研究表明,GH4169合金在NaCl盐雾和固态NaCl + 含O2水蒸汽环境下的腐蚀增重均明显增加,且后者的腐蚀速率显著大于前者。GH4169合金在NaCl盐雾环境下的腐蚀产物主要为Cr2O3、Fe2O3、NiFe2O4和NaNbO3,其腐蚀层较为致密,且氯在内腐蚀层中富集。在NaCl盐雾环境下,腐蚀初期GH4169合金以氧化和氯的活性氧化机理共同作用加速腐蚀,随着NaCl沉积量的增加合金腐蚀逐渐变为以氯的活性氧化机制为主的加速腐蚀。此外,对GH4169合金的主要元素及其氧化物在中温NaCl盐雾环境下的反应敏感性进行了计算分析,结果表明,NaCl盐雾环境下GH4169合金内各元素对氯活化腐蚀敏感性的排序依次为:Ti > Al > Nb、Cr > Fe >Mo、Ni,合金氧化物对环境的敏感性顺序为:TiO2 > MoO2 > Cr2O3(Nb2O5) > Fe2O3 > Al2O3 > NiO。

关键词 : GH4169合金,  NaCl盐雾,  合金元素敏感性    
Abstract:

The corrosion behavior of engine materials of airplanes working in marine environments is accelerated by the synergistic effects of NaCl particles and water vapor at high temperatures. This work examined the corrosion behavior of GH4169 alloy with a NaCl solution spraying at 600oC using an oxidation kinetics test and micro characterization technology in the aspects of corrosion kinetics, corrosion layer phase composition, and microstructure. The weight gain of the GH4169 alloy corroded in the NaCl solution spraying environment was much lower than that in solid NaCl + wet O2 after 20 h corrosion at 600oC. The corrosion products of the GH4169 alloy in the NaCl solution spray environment were less complex than those in the solid NaCl + wet O2 environment, but they were denser. In addition, Cl was concentrated in the inner layer of the corrosion products and accelerated the corrosion of GH4169 alloy via an “active oxidation” mechanism at the initial stage. When NaCl deposition was increased, the corrosion mechanism of GH4169 alloy changed gradually to Cl-induced “active oxidation.” The sensitivity of GH4169 alloy in the NaCl solution spray environment at 600oC was analyzed. Overall, the sensitivity of elements in GH4169 alloy to chlorine activated corrosion was Ti > Al > Nb, Cr > Fe > Mo, Ni, whereas the sensitivity of the oxides was TiO2 > MoO2 > Cr2O3(Nb2O5) > Fe2O3 > Al2O3 > NiO.

Key words: GH4169 alloy    NaCl solution spray    sensitivity of alloy element
收稿日期: 2022-04-29     
ZTFLH:  TG174  
基金资助:国家自然科学基金企业创新联合基金重点项目(U20B2026)
通讯作者: 刘 莉,liuli@mail.neu.edu.cn,主要从事腐蚀电化学、金属腐蚀与防护方面的研究;
崔 宇,ycui@imr.ac.cn,主要从事海洋中温环境金属腐蚀与防护研究
Corresponding author: LIU Li, professor, Tel: 15904072057, E-mail: liuli@mail.neu.edu.cn;
CUI Yu, associate researcher, Tel: 15004059681, E-mail: ycui@imr.ac.cn
作者简介: 张伟东,男,1989年生,博士
图1  中温NaCl盐雾和固态NaCl + 含O2水蒸汽腐蚀模拟装置示意图
图2  GH4169合金在600℃的纯O2、含O2水蒸汽、固态NaCl + 含O2水蒸汽和NaCl盐雾环境下腐蚀 20 h的腐蚀动力学曲线
图3  GH4169合金在600℃的固态NaCl + 含O2水蒸汽和NaCl盐雾环境服役5 min后表面SEM像
图4  GH4169合金在600℃纯O2、含O2水蒸汽、固态NaCl + 含O2水蒸汽和NaCl盐雾环境下腐蚀20 h后的表面SEM像
PointCrNiNaAlTiFeNbO
135.542.13--0.020.050.0362.23
229.831.35-0.030.031.030.0667.67
33.373.100.070.020.0459.930.1033.37
42.311.4222.250.020.951.0723.1449.91
515.6115.581.820.730.6510.532.7152.37
表1  图4中各点的EDS结果 (mass fraction / %)
图5  GH4169合金在600℃纯O2、含O2水蒸汽、固态NaCl + 含O2水蒸汽和NaCl盐雾环境腐蚀20 h后的截面SEM像
图6  GH4169合金在600℃纯O2、含O2水蒸汽、固态NaCl + 含O2水蒸汽和NaCl盐雾环境下腐蚀20 h的XRD谱
图7  GH4169合金在600℃固态NaCl + 含O2水蒸汽和NaCl盐雾环境下腐蚀20 h后截面的EPMA元素面分布图
图8  GH4169合金在600℃的NaCl盐雾环境中腐蚀100 h后截面的EPMA元素面分布图
图9  GH4169合金在600℃下NaCl盐雾环境腐蚀20 h后腐蚀产物膜的TEM像、SAED花样及Cl元素线分布结果
图10  GH4169合金在600℃固态NaCl + 含O2水蒸汽环境腐蚀 20 h后内腐蚀区域的TEM像及EDS结果
ReactionΔG0 / (kJ·mol-1)
4NaCl (g) + O2 (g) + 2TiO2 = 2Na2TiO3 + 2Cl2 (g)-133.57
4NaCl (g) + 2H2O (g) + TiO2 = 2Na2TiO3 + 4HCl (g)-64.06
4NaCl (g) + 2Al2O3 + 2H2O (g) = 4NaAlO2 + 4HCl (g)280.4
4NaCl (g) + 2Al2O3 + O2 (g) = 4NaAlO2 + 2Cl2 (g)174.2
4NaCl (g) + 2Fe2O3 + O2 (g) = 4NaFeO2 + 2Cl2 (g)4
4NaCl (g) + 2Fe2O3 + 2H2O (g) = 4NaFeO2 + 4HCl (g)3.8
4NaCl (g) + Cr2O3 + 2H2O (g) + 3/2O2 (g) = 2Na2CrO4 + 4HCl (g)-54.5
4NaCl (g) + Cr2O3 + 5/2O2 (g) = 2Na2CrO4 + 2Cl2 (g)-54.4
4NaCl (g) + 4NiO + O2 + 2H2O = 4NaNiO2 + 4HCl (g)-
4NaCl (g) + 2Nb2O5 + O2 (g) = 4NaNbO3 + 2Cl2 (g)-
4NaCl (g) + 2H2O (g) + 2MoO2 + O2 (g) = 2Na2MoO4 + 4HCl (g)-115.6
表2  相关化学反应在600℃时的标准Gibbs自由能
图11  M-Cl-O体系在600℃时以lgpO2和lgpCl为坐标的平衡图
1 Wang C, Jiang F, Wang F. Corrosion inhibition of 304 stainless steel by nano-sized Ti/silicone coatings in an environment containing NaCl and water vapor at 400-600oC [J]. Oxid. Met., 2004, 62: 1
doi: 10.1023/B:OXID.0000038782.77162.5b
2 Shu Y H, Wang F H, Wu W T. Synergestic effect of NaCl and water vapor on the corrosion of Ti60 alloy at 500-700oC [J]. Oxid. Met., 1999, 52: 463
doi: 10.1023/A:1018864216554
3 Shu Y H, Wang F H, Wu W T. Synergistic effect of NaCl and water vapor on the corrosion of 1Cr-11Ni-2W-2Mo-V steel at 500-700oC [J]. Oxid. Met., 1999, 51: 97
doi: 10.1023/A:1018854202982
4 Shu Y H, Wang F H, Wu W T. Corrosion behavior of pure Cr with a solid NaCl deposit in O2 plus water vapor [J]. Oxid. Met., 2000, 54: 457
doi: 10.1023/A:1004690518225
5 Wang F H, Geng S J, Zhu S L. Corrosion behavior of a sputtered K38G nanocrystalline coating with a solid NaCl deposit in wet oxygen at 600 to 700oC [J]. Oxid. Met., 2002, 58: 185
doi: 10.1023/A:1016072726338
6 Wang F, Shu Y. Influence of Cr content on the corrosion of Fe-Cr alloys: The synergistic effect of NaCl and water vapor [J]. Oxid. Met., 2003, 59: 201
doi: 10.1023/A:1023083309041
7 Grabke H J, Reese E, Spiegel M. The effects of chlorides, hydrogen chloride, and sulfur dioxide in the oxidation of steels below deposits [J]. Corros. Sci., 1995, 37: 1023
doi: 10.1016/0010-938X(95)00011-8
8 Liu L, Li Y, Zeng C L, et al. Electrochemical impedance spectroscopy (EIS) studies of the corrosion of pure Fe and Cr at 600oC under solid NaCl deposit in water vapor [J]. Electrochim. Acta, 2006, 51: 4736
doi: 10.1016/j.electacta.2006.01.033
9 Tang Y B, Liu L, Li Y, et al. The electrochemical corrosion mechanisms of pure Cr with NaCl deposit in water vapor at 600oC [J]. J. Electrochem. Soc., 2011, 158: C237
doi: 10.1149/1.3596167
10 Fan L, Liu L, Cao M, et al. Corrosion behavior of pure Ti under a solid NaCl deposit in a wet oxygen flow at 600oC [J]. Metals, 2016, 6: 72
doi: 10.3390/met6040072
11 Fan L, Liu L, Yu Z F, et al. Corrosion behavior of Ti60 alloy under a solid NaCl deposit in wet oxygen flow at 600oC [J]. Sci. Rep, 2016, 6: 29019
doi: 10.1038/srep29019
12 Ciszak C, Abdallah I, Popa I, et al., Degradation mechanism of Ti-6Al-2Sn-4Zr-2Mo-Si alloy exposed to solid NaCl deposit at high temperature [J]. Corros. Sci., 2020, 172: 108611
doi: 10.1016/j.corsci.2020.108611
13 Folkeson N, Jonsson T, Halvarsson M, et al., The influence of small amounts of KCl(s) on the high temperature corrosion of a Fe-2.25Cr-1Mo steel at 400 and 500oC [J]. Mater. Corros., 2011, 62: 606
14 Cao M, Liu L, Yu Z F, et al. Studies on the corrosion behavior of Fe-20Cr alloy in NaCl solution spray at 600oC [J]. Corros. Sci., 2018, 133: 165
doi: 10.1016/j.corsci.2018.01.033
15 Li R, Cui Y, Liu L, et al. Corrosion behavior of Ti60 alloy in fog of NaCl solution at 600oC [J]. J. Chin. Soc. Corros. Prot., 2021, 41: 595
15 李 蕊, 崔 宇, 刘 莉 等. NaCl盐雾环境下Ti60合金的中温腐蚀行为 [J]. 中国腐蚀与防护学报, 2021, 41: 595
16 Mahobia G S, Paulose N, Singh V. Hot corrosion behavior of superalloy IN718 at 550 and 650oC [J]. J. Mater. Eng. Perform., 2013, 22: 2418
doi: 10.1007/s11665-013-0532-0
17 Pradhan D G, Mahobia G S, Chattopadhyay K, et al. Salt induced corrosion behaviour of superalloy IN718 [J]. Mater. Today Proc., 2018, 5: 7047
18 Shen M L, Zhu S L, Wang F H. Cyclic oxidation behavior of glass-ceramic composite coatings on superalloy K38G at 1100oC [J]. Thin Solid Films, 2011, 519: 4884
doi: 10.1016/j.tsf.2011.01.047
19 Yu Z F, Liu L, Liu R, et al. Corrosion behavior of GH4169 alloy under alternating oxidation at 900oC and solution immersion [J]. Materials (Basel), 2019, 12: 1503
doi: 10.3390/ma12091503
20 Pradhan D, Mahobia G S, Chattopadhyay K, et al. Severe hot corrosion of the superalloy IN718 in mixed salts of Na2SO4 and V2O5 at 700oC [J]. J. Mater. Eng. Perform., 2018, 27: 4235
doi: 10.1007/s11665-018-3501-9
21 Sun W Y, Wang J L, Yang L L, et al. Studies on corrosion behavior of a single-crystal superalloy and its sputtered nanocrystalline coatings with solid NaCl deposit in O2 + 38 vol.% H2O environment at 700oC [J]. Corros. Sci., 2019, 161: 108187
doi: 10.1016/j.corsci.2019.108187
22 Xu S, Long F, Persaud S Y, et al. Oxidation behavior of 9Cr-4.5Al ODS steel in 600oC supercritical water and the effect of pre-oxidation [J]. Corros. Sci., 2020, 165: 108380
doi: 10.1016/j.corsci.2019.108380
23 Zhuang X P, Tan Y, You X G, et al. High temperature oxidation behavior and mechanism of a new Ni-Co-based superalloy [J]. Vacuum, 2021, 189: 110219
doi: 10.1016/j.vacuum.2021.110219
24 Jonsson T, Pujilaksono B, Heidari H, et al. Oxidation of Fe-10Cr in O2 and in O2 + H2O environment at 600oC: A microstructural investigation [J]. Corros. Sci., 2013, 75: 326
doi: 10.1016/j.corsci.2013.06.016
25 Juez-Lorenzo M, Kolarik V, Stamm W, et al. Oxidation of nickel-based alloys in dry and water vapour containing air [J]. Mater. High Temp., 2012, 29: 229
doi: 10.3184/096034012X13348393336892
26 Israelsson N, Hellström K, Svensson J E, et al. KCl-induced corrosion of the FeCrAl alloy Kanthal® AF at 600oC and the effect of H2O [J]. Oxid. Met., 2015, 83: 1
doi: 10.1007/s11085-014-9506-3
27 Israelsson N, Engkvist J, Hellström K, et al. KCl-induced corrosion of an FeCrAl alloy at 600oC in O2 + H2O environment: The effect of pre-oxidation [J]. Oxid. Met., 2015, 83: 29
doi: 10.1007/s11085-014-9507-2
28 Fan L. Investigation on corrosion behavior of Ti60 alloy under synergetic effect of solid NaCl deposit and water vapor at 600oC [D]. Shenyang: University of Chinese Academy of Sciences (Institute of Metal Research, Chinese Academy of Scionces), 2016
28 范 磊. 固态NaCl和水蒸汽协同作用下Ti60合金中温腐蚀行为的研究 [D]. 沈阳: 中国科学院大学(中国科学院金属研究所), 2016
29 Wang W Q, Cui Y, Liu R, et al. Revealing internal corrosion of GH4169 with stress coupled solid NaCl deposited in a humid environment of 600oC [J]. Corros. Sci., 2022, 195: 110004
doi: 10.1016/j.corsci.2021.110004
30 Phother-Simon J, Hanif I, Liske J, et al. The influence of a KCl-rich environment on the corrosion attack of 304 L: 3D FIB/SEM and TEM investigations [J]. Corros. Sci., 2021, 183: 109315
doi: 10.1016/j.corsci.2021.109315
31 Israelsson N, Unocic K A, Hellström K, et al. Cyclic corrosion and chlorination of an FeCrAl alloy in the presence of KCl [J]. Oxid. Met., 2015, 84: 269
doi: 10.1007/s11085-015-9554-3
32 Israelsson N, Unocic K A, Hellström K, et al. A microstructural and kinetic investigation of the KCl-induced corrosion of an FeCrAl alloy at 600oC [J]. Oxid. Met., 2015, 84: 105
doi: 10.1007/s11085-015-9546-3
[1] 杜金辉, 毕中南, 曲敬龙. 三联冶炼GH4169合金研究进展[J]. 金属学报, 2023, 59(9): 1159-1172.
[2] 李彦默, 郭小辉, 陈斌, 李培跃, 郭倩颖, 丁然, 余黎明, 苏宇, 李文亚. GH4169合金与S31042钢线性摩擦焊接头组织及力学性能[J]. 金属学报, 2021, 57(3): 363-374.
[3] 王磊, 安金岚, 刘杨, 宋秀. 多场耦合作用下GH4169合金变形行为与强韧化机制[J]. 金属学报, 2019, 55(9): 1185-1194.
[4] 王建国,刘东,杨艳慧. GH4169合金非均匀组织在加热过程中的演化机理*[J]. 金属学报, 2016, 52(6): 707-716.
[5] 安金岚,王磊,刘杨,胥国华,赵光普. 长期时效对GH4169合金组织演化及低周疲劳行为的影响*[J]. 金属学报, 2015, 51(7): 835-843.
[6] 王磊,安金岚,刘杨,宋秀,胥国华,赵光普. 静电场处理对GH4169合金中d相析出行为的影响[J]. 金属学报, 2015, 51(10): 1235-1241.
[7] 刘奋成, 林鑫, 余小斌, 黄春平, 黄卫东. 激光立体成形GH4169合金再结晶过程中的界面和晶体取向演化*[J]. 金属学报, 2014, 50(4): 463-470.
[8] 张海燕,张士宏,程明. δ相对GH4169合金高温拉伸变形行为的影响[J]. 金属学报, 2013, 29(4): 483-488.
[9] 张麦仓,曹国鑫,董建新,郑磊,姚志浩. 基于经典动态模型的GH4169合金钢锭中Laves相的回溶规律分析[J]. 金属学报, 2013, 49(3): 372-378.
[10] 刘杨 王磊 何思斯 冯飞 吕旭东 张北江. 长期时效对GH4169合金动态拉伸变形行为的影响[J]. 金属学报, 2012, 48(1): 49-55.