| 金属塑性成形的应变路径效应:机制、表征与应用 |
樊晓光1,2,3, 肖云腾1,2, 詹梅1,2( ), 马飞1,2, 高鹏飞1,2, 郑泽邦1,2, 张昕2,3, 邵光大2,4, 伍寓铭1,2 |
1 西北工业大学 材料学院 西安 710072 2 西北工业大学 陕西省高性能精确成形技术与装备重点实验室 西安 710072 3 西北工业大学 航空发动机高性能制造工业和信息化部重点实验室 西安 710072 4 上海交通大学 上海市复杂薄板结构数字化制造重点实验室 上海 200240 |
|
| Strain Path Effects in Metal Plastic Forming: Mechanisms, Characterization, and Application |
FAN Xiaoguang1,2,3, XIAO Yunteng1,2, ZHAN Mei1,2( ), MA Fei1,2, GAO Pengfei1,2, ZHENG Zebang1,2, ZHANG Xin2,3, SHAO Guangda2,4, WU Yuming1,2 |
1 School of Materials Science and Engineering, Northwestern Polytechnical University, Xi'an 710072, China 2 Shaanxi Key Laboratory of High-Performance Precision Forming Technology and Equipment, Northwestern Polytechnical University, Xi'an 710072, China 3 Key Laboratory of High Performance Manufacturing for Aero Engine, Ministry of Industry and Information Technology, Northwestern Polytechnical University, Xi'an 710072, China 4 Shanghai Key Laboratory of Digital Manufacture for Thin-Walled Structures, Shanghai Jiao Tong University, Shanghai 200240, China |
引用本文:
樊晓光, 肖云腾, 詹梅, 马飞, 高鹏飞, 郑泽邦, 张昕, 邵光大, 伍寓铭. 金属塑性成形的应变路径效应:机制、表征与应用[J]. 金属学报, 2026, 62(5): 975-992.
Xiaoguang FAN,
Yunteng XIAO,
Mei ZHAN,
Fei MA,
Pengfei GAO,
Zebang ZHENG,
Xin ZHANG,
Guangda SHAO,
Yuming WU.
Strain Path Effects in Metal Plastic Forming: Mechanisms, Characterization, and Application[J]. Acta Metall Sin, 2026, 62(5): 975-992.
| [1] |
Yang H. Local Loading Control of Nonuniform Deformation and Precise Plastic Forming: Principles and Techniques [M]. Beijing: Science Press, 2014: 1
|
| [1] |
杨 合. 局部加载控制不均匀变形与精确塑性成形: 原理和技术 [M]. 北京: 科学出版社, 2014: 1
|
| [2] |
Lin Z Q, Huang Q X, Yuan S J, et al. Major breakthrough and progress in metal forming technology and equipment of China in the last 30 years [J]. J. Plast. Eng., 2024, 31(4): 2
|
| [2] |
林忠钦, 黄庆学, 苑世剑 等. 中国塑性成形技术和装备30年的重大突破与进展 [J]. 塑性工程学报, 2024, 31(4): 2
|
| [3] |
Schmitt J H, Shen E L, Raphanel J L. A parameter for measuring the magnitude of a change of strain path: Validation and comparison with experiments on low carbon steel [J]. Int. J. Plast., 1994, 10: 535
doi: 10.1016/0749-6419(94)90013-2
|
| [4] |
Dunand M, Maertens A P, Luo M, et al. Experiments and modeling of anisotropic aluminum extrusions under multi-axial loading—Part I: Plasticity [J]. Int. J. Plast., 2012, 36: 34
doi: 10.1016/j.ijplas.2012.03.003
|
| [5] |
Shi B D, Shi R, Zhao H, et al. Review on deformation behavior of sheet metal during biaxial compression [J]. Forg. Stamp. Technol., 2024, 49(7): 19
|
| [5] |
石宝东, 石 瑞, 赵 辉 等. 金属板材双轴压缩变形行为研究进展 [J]. 锻压技术, 2024, 49(7): 19
|
| [6] |
Jiang X Q, Fan X G, Zhan M, et al. Research progress on plastic flow instability during hot deformation of metal materials [J]. J. Plast. Eng., 2020, 27(7): 33
|
| [6] |
姜雪琦, 樊晓光, 詹 梅 等. 金属材料热变形中的塑性流动失稳研究进展 [J]. 塑性工程学报, 2020, 27(7): 33
doi: 10.3969/j.issn.1007-2012.2020.07.005
|
| [7] |
Gautam P C, Al-Samman T, Thangaraju S, et al. Effect of ECAP strain path on deformation behaviour, microstructure, texture evolution, and mechanical properties in magnesium [J]. Mater. Sci. Eng., 2024, A913: 147077
|
| [8] |
Bharti A, Dey R, Sivaprasad S, et al. Deformation response and microstructure evolution in 304LN stainless steel subjected to multiaxial fatigue loading under different strain paths [J]. Int. J. Press. Vessels Pip., 2025, 214: 105452
doi: 10.1016/j.ijpvp.2025.105452
|
| [9] |
Dhara S, Taylor S, Figiel Ł, et al. Development of a novel testing methodology for in-situ microstructural characterisation during continuous strain path change [J]. Mater. Charact., 2022, 183: 111610
doi: 10.1016/j.matchar.2021.111610
|
| [10] |
Jiang X Q. Study on the correlation between strain localization and microstructure of TA15 titanium alloy and its prediction [D]. Xi’an: Northwestern Polytechnical University, 2021
|
| [10] |
姜雪琦. TA15钛合金应变局部化的组织相关性与预测研究 [D]. 西安: 西北工业大学, 2021
|
| [11] |
Xie Z X, Fan X G, Wang L, et al. Stepwise cooling spinning to achieve isotropic strength-ductility synergy of titanium alloy tube [J]. J. Mater. Sci. Technol., 2026, 244: 156
doi: 10.1016/j.jmst.2025.03.106
|
| [12] |
Li H W, Gao J, Sun X X, et al. Research developments on multiscale modeling and simulation towards high-performance plastic forming [J]. J. Mech. Eng., 2024, 60(1): 27
|
| [12] |
李宏伟, 高 佳, 孙新新 等. 面向高性能塑性成形的多尺度建模仿真研究进展 [J]. 机械工程学报, 2024, 60(1): 27
|
| [13] |
Zhao T Z, Zhang S H, Cheng M, et al. Development of strain path effects on the mechanical behaviors of metals [J]. Forg. Stamp. Technol., 2016, 41(10): 1
|
| [13] |
赵天章, 张士宏, 程 明 等. 金属力学行为中应变路径效应的研究进展 [J]. 锻压技术, 2016, 41(10): 1
|
| [14] |
Boger R K, Wagoner R H, Barlat F, et al. Continuous, large strain, tension/compression testing of sheet material [J]. Int. J. Plast., 2005, 21: 2319
doi: 10.1016/j.ijplas.2004.12.002
|
| [15] |
Liao J, Xue X, Lee M G, et al. Constitutive modeling for path-dependent behavior and its influence on twist springback [J]. Int. J. Plast., 2017, 93: 64
doi: 10.1016/j.ijplas.2017.02.009
|
| [16] |
Van Petegem S, Wagner J, Panzner T, et al. In-situ neutron diffraction during biaxial deformation [J]. Acta Mater., 2016, 105: 404
doi: 10.1016/j.actamat.2015.12.015
|
| [17] |
Zhan M, Dong Y D, Zhai Z L, et al. Review on fast numerical simulation method for plastic forming [J]. J. Mech. Eng., 2022, 58(16): 2
doi: 10.3901/JME.2022.16.002
|
| [17] |
詹 梅, 董赟达, 翟卓蕾 等. 塑性成形快速数值仿真方法的研究进展 [J]. 机械工程学报, 2022, 58(16): 2
|
| [18] |
Guo S Q, Yan S L, Huang L, et al. A strain-path dependent unified constitutive model of titanium alloy coupling coarse grain subdivision and recrystallization: Application to multi-directional hot deformation [J]. Int. J. Plast., 2025, 186: 104248
doi: 10.1016/j.ijplas.2025.104248
|
| [19] |
Fan R L, Chen M H, Wu D P, et al. Research progress of forming limit of sheet metal under nonlinear loading path [J]. J. Plast. Eng., 2024, 31(2): 1
|
| [19] |
范荣磊, 陈明和, 吴迪鹏 等. 非线性加载路径下金属薄板成形极限研究进展 [J]. 塑性工程学报, 2024, 31(2): 1
|
| [20] |
Yang B, Zhang W G, Lin Z Q, et al. The study of loading path optimization for tube hydroforming process [J]. J. Plast. Eng., 2006, 13(4): 10
|
| [20] |
杨 兵, 张卫刚, 林忠钦 等. 管件液压成形中加载路径的优化设计方法研究 [J]. 塑性工程学报, 2006, 13(4): 10
|
| [21] |
Sharma R, Sargeant D, Daroju S, et al. Multi-strain path deformation behavior of AA6016-T4: Experiments and crystal plasticity modeling [J]. Int. J. Solids Struct., 2022, 244-245: 111536
doi: 10.1016/j.ijsolstr.2022.111536
|
| [22] |
Daroju S, Kuwabara T, Sharma R, et al. Experimental characterization and crystal plasticity modeling for predicting load reversals in AA6016-T4 and AA7021-T79 [J]. Int. J. Plast., 2022, 153: 103292
doi: 10.1016/j.ijplas.2022.103292
|
| [23] |
Li F, Zhang H Y, He W W, et al. Compression and tensile consecutive deformation behavior of Mn18Cr18N austenite stainless steel [J]. Acta Metall. Sin., 2016, 52: 956
doi: 10.11900/0412.1961.2015.00547
|
| [23] |
李 飞, 张华煜, 何文武 等. Mn18Cr18N奥氏体不锈钢的压缩拉伸连续加载变形行为 [J]. 金属学报, 2016, 52: 956
|
| [24] |
Xu S, Liu T M, Ding X Z, et al. Reducing the anisotropy of a pre-twinned hot-rolled Mg-3Al-1Zn alloy by plane-strain compression [J]. Mater. Sci. Eng., 2014, A592: 230
|
| [25] |
Shi B D, Peng Y, Yang C, et al. Loading path dependent distortional hardening of Mg alloys: Experimental investigation and constitutive modeling [J]. Int. J. Plast., 2017, 90: 76
doi: 10.1016/j.ijplas.2016.12.006
|
| [26] |
Zhang Z X, Qu S J, Feng A H, et al. Microstructural mechanisms during multidirectional isothermal forging of as-cast Ti-6Al-4V alloy with an initial lamellar microstructure [J]. J. Alloys Compd., 2019, 773: 277
doi: 10.1016/j.jallcom.2018.09.220
|
| [27] |
Hama T, Nagao H, Kobuki A, et al. Work-hardening and twinning behaviors in a commercially pure titanium sheet under various loading paths [J]. Mater. Sci. Eng., 2015, A620: 390
|
| [28] |
Wroński M, Kumar M A, McCabe R J, et al. Deformation behavior of CP-titanium under strain path changes: Experiment and crystal plasticity modeling [J]. Int. J. Plast., 2022, 148: 103129
doi: 10.1016/j.ijplas.2021.103129
|
| [29] |
Hou Y, Lee M G, Lin J P, et al. Experimental characterization and modeling of complex anisotropic hardening in quenching and partitioning (Q&P) steel subject to biaxial non-proportional loadings [J]. Int. J. Plast., 2022, 156: 103347
doi: 10.1016/j.ijplas.2022.103347
|
| [30] |
Benzerga A A, Surovik D, Keralavarma S M. On the path-dependence of the fracture locus in ductile materials-Analysis [J]. Int. J. Plast., 2012, 37: 157
doi: 10.1016/j.ijplas.2012.05.003
|
| [31] |
Cortese L, Nalli F, Rossi M. A nonlinear model for ductile damage accumulation under multiaxial non-proportional loading conditions [J]. Int. J. Plast., 2016, 85: 77
doi: 10.1016/j.ijplas.2016.07.003
|
| [32] |
Zhang R, Xu Z T, Deng Y J, et al. Characterizing the back stress of ultra-thin metallic sheet via pre-strain tension/bending process [J]. J. Mater. Process. Technol., 2020, 279: 116560
doi: 10.1016/j.jmatprotec.2019.116560
|
| [33] |
Fincato R, Tsutsumi S. Numerical modeling of the evolution of ductile damage under proportional and non-proportional loading [J]. Int. J. Solids Struct., 2019, 160: 247
doi: 10.1016/j.ijsolstr.2018.10.028
|
| [34] |
Itoh T, Yang T. Material dependence of multiaxial low cycle fatigue lives under non-proportional loading [J]. Int. J. Fatigue, 2011, 33: 1025
doi: 10.1016/j.ijfatigue.2010.12.001
|
| [35] |
Yu J W, Fan X G, Wang L, et al. Mechanism of the high elongation but low formability of high-strength aluminum alloy in W-temper [J]. J. Mater. Process. Technol., 2025, 345: 119068
doi: 10.1016/j.jmatprotec.2025.119068
|
| [36] |
Wollenweber M A, Medghalchi S, Guimarães L R, et al. On the damage behaviour in dual-phase DP800 steel deformed in single and combined strain paths [J]. Mater. Des., 2023, 231: 112016
doi: 10.1016/j.matdes.2023.112016
|
| [37] |
Marcadet S J, Mohr D. Effect of compression-tension loading reversal on the strain to fracture of dual phase steel sheets [J]. Int. J. Plast., 2015, 72: 21
doi: 10.1016/j.ijplas.2015.05.002
|
| [38] |
Yu K, Yoon J W. Characterization of compressive fracture strain based on bilinear strain paths [J]. Int. J. Plast., 2024, 183: 104168
doi: 10.1016/j.ijplas.2024.104168
|
| [39] |
Sanderson S G, Najmabad S I, Sharma R, et al. Observation and modeling of strain gradients in AA6016—Influence of length-scale, microstructure, and strain path [J]. Mater. Charact., 2025, 222: 114843
doi: 10.1016/j.matchar.2025.114843
|
| [40] |
Wang Z S, Wang T, Guan Y J, et al. Effect of strain path on microstructure and mechanical properties of AZ31 magnesium alloy sheets processed by constrained groove pressing [J]. Mater. Sci. Eng., 2021, A804: 140794
|
| [41] |
Poths R M, Angella G, Wynne B P, et al. Effect of strain reversal on the dynamic spheroidization of Ti-6Al-4V during hot deformation [J]. Metall. Mater. Trans., 2004, 35A: 2993
|
| [42] |
Zhao A M, Yang H, Fan X G, et al. The flow behavior and microstructure evolution during (α + β) deformation of β wrought TA15 titanium alloy [J]. Mater. Des., 2016, 109: 112
doi: 10.1016/j.matdes.2016.07.001
|
| [43] |
Wang L, Fan X G, Zhan M, et al. Experimental characterization and physical modeling of strain path dependent microstructure evolution: A case study of primary hot working of titanium alloy [J]. Int. J. Plast., 2022, 158: 103450
doi: 10.1016/j.ijplas.2022.103450
|
| [44] |
Huang Z, Luo S, Wang G Y, et al. Mechanistic exploration of high strain-hardening and TWIP effects in Fe-15.5Mn-0.6C-1.4Al steel under compression-tensile loading [J]. Int. J. Plast., 2025, 188: 104292
doi: 10.1016/j.ijplas.2025.104292
|
| [45] |
Xin Y C, Jiang J, Chapuis A, et al. Plastic deformation behavior of AZ31 magnesium alloy under multiple passes cross compression [J]. Mater. Sci. Eng., 2012, A532: 50
|
| [46] |
Yang H, Zhou G W, Wang H M, et al. Experimental and numerical study on strain path and crystal orientation dependences of phase transformation behaviors of QP1180 steel [J]. Int. J. Plast., 2023, 160: 103499
doi: 10.1016/j.ijplas.2022.103499
|
| [47] |
Sahoo S K, Sabat R K, Sahni S, et al. Texture and microstructure evolution of commercially pure titanium during hot rolling: Role of strain-paths [J]. Mater. Des., 2016, 91: 58
doi: 10.1016/j.matdes.2015.11.073
|
| [48] |
Gupta A, Khatirkar R K, Dandekar T, et al. Texture development during multi-step cross rolling of a β titanium alloy: Experiments and simulation [J]. J. Alloys Compd., 2021, 850: 156824
doi: 10.1016/j.jallcom.2020.156824
|
| [49] |
Fan J K, Zhao D, Chen Z S, et al. Tailoring texture in a near-α titanium alloy: Insights from strain paths and cooling rate influences [J]. J. Mater. Res. Technol., 2024, 30: 1388
doi: 10.1016/j.jmrt.2024.03.151
|
| [50] |
Tang L Q, Jiang F L, Teng J, et al. Strain path dependent evolutions of microstructure and texture in AZ80 magnesium alloy during hot deformation [J]. J. Alloys Compd., 2019, 806: 292
doi: 10.1016/j.jallcom.2019.07.262
|
| [51] |
Li Y Y, Han T Z, Chu Z B, et al. Effect of strain path on mechanical behavior of AZ31 magnesium alloy [J]. Rare Met. Mater. Eng., 2022, 51: 2785
|
| [52] |
Wu W J, Chen W Z, Wang X Y, et al. Texture adjustment approach of magnesium alloys via variable strain path calculated by an integrated finite element-viscoplastic self-consistent model [J]. J. Mater. Sci. Technol., 2024, 184: 15
doi: 10.1016/j.jmst.2023.09.054
|
| [53] |
El-Danaf E A. Mechanical properties, microstructure and micro-texture evolution for 1050AA deformed by equal channel angular pressing (ECAP) and post ECAP plane strain compression using two loading schemes [J]. Mater. Des., 2012, 34: 793
doi: 10.1016/j.matdes.2011.07.006
|
| [54] |
Dhara S, Hughes D J, Huband S, et al. An X-ray diffraction study of the influence of linear and changing strain paths on strain and texture evolution in AA6111-T4 aluminium alloy sheets [J]. Materialia, 2024, 38: 102305
doi: 10.1016/j.mtla.2024.102305
|
| [55] |
Zeng X, Fan X G, Li H W, et al. Grain refinement in hot working of 2219 aluminium alloy: On the effect of deformation mode and loading path [J]. Mater. Sci. Eng., 2020, A794: 139905
|
| [56] |
Collins D M, Erinosho T, Dunne F P E, et al. A synchrotron X-ray diffraction study of non-proportional strain-path effects [J]. Acta Mater., 2017, 124: 290
doi: 10.1016/j.actamat.2016.11.011
|
| [57] |
Akbarian S H, Zarei-Hanzaki A, Anoushe A S, et al. Step-by-step texture modification through strain path change toward improvement of the hardening capacity in a twinning-induced-plasticity steel [J]. Mater. Sci. Eng., 2021, A799: 140269
|
| [58] |
Shaabani A, Jamaati R, Hosseinipour S J. Effect of strain path and short-term post-annealing on the microstructure, texture, and mechanical anisotropy of low-carbon steel [J]. Mater. Charact., 2024, 215: 114148
doi: 10.1016/j.matchar.2024.114148
|
| [59] |
Fan X G, Jiang X Q, Zeng X, et al. Modeling the anisotropy of hot plastic deformation of two-phase titanium alloys with a colony microstructure [J]. Int. J. Plast., 2018, 104: 173
doi: 10.1016/j.ijplas.2018.02.010
|
| [60] |
Chen F, Tian X, Liu Z X, et al. A novel continuous dynamic recrystallization model to reveal grain refinement mechanism in constraining ring rolling of thin-walled conical structure with inner ribs [J]. Int. J. Mach. Tools Manuf., 2025, 206: 104255
doi: 10.1016/j.ijmachtools.2025.104255
|
| [61] |
Wei D L, Cui Z S, Chen J. Optimization and tolerance prediction of sheet metal forming process using response surface model [J]. Comput. Mater. Sci., 2008, 42: 228
doi: 10.1016/j.commatsci.2007.07.014
|
| [62] |
Yang H, Tang W Q, Li D Y. Development and verification of crystal plasticity finite element model considering phase transformation [J]. J. Plast. Eng., 2025, 32(4): 169
|
| [62] |
杨 浩, 唐伟琴, 李大永. 考虑相变的晶体塑性有限元模型开发及验证 [J]. 塑性工程学报, 2025, 32(4): 169
|
| [63] |
Liu R X, Li K, Zhou G W, et al. Simulation of strain induced abnormal grain growth in aluminum alloy by coupling crystal plasticity and phase field methods [J]. Trans. Nonferrous Met. Soc. China, 2022, 32: 3873
doi: 10.1016/S1003-6326(22)66064-3
|
| [64] |
Barlat F, Brem J C, Yoon J W, et al. Plane stress yield function for aluminum alloy sheets—part 1: Theory [J]. Int. J. Plast., 2003, 19: 1297
doi: 10.1016/S0749-6419(02)00019-0
|
| [65] |
Yoon J W, Barlat F, Dick R E, et al. Plane stress yield function for aluminum alloy sheets-part II: FE formulation and its implementation [J]. Int. J. Plast., 2004, 20: 495
doi: 10.1016/S0749-6419(03)00099-8
|
| [66] |
Deng N X, Kuwabara T, Korkolis Y P. On the non-linear unloading behavior of a biaxially loaded dual-phase steel sheet [J]. Int. J. Mech. Sci., 2018, 138-139: 383
doi: 10.1016/j.ijmecsci.2018.02.015
|
| [67] |
Hou Y, Min J Y, Guo N, et al. Investigation of evolving yield surfaces of dual-phase steels [J]. J. Mater. Process. Technol., 2021, 287: 116314
doi: 10.1016/j.jmatprotec.2019.116314
|
| [68] |
Chaboche J L. Constitutive equations for cyclic plasticity and cyclic viscoplasticity [J]. Int. J. Plast., 1989, 5: 247
doi: 10.1016/0749-6419(89)90015-6
|
| [69] |
Haddag B, Balan T, Abed-Meraim F. Investigation of advanced strain-path dependent material models for sheet metal forming simulations [J]. Int. J. Plast., 2007, 23: 951
doi: 10.1016/j.ijplas.2006.10.004
|
| [70] |
Barlat F, Ha J J, Grácio J J, et al. Extension of homogeneous anisotropic hardening model to cross-loading with latent effects [J]. Int. J. Plast., 2013, 46: 130
doi: 10.1016/j.ijplas.2012.07.002
|
| [71] |
Yang Y F, Balan T. Prediction of the yield surface evolution and some apparent non-normality effects after abrupt strain-path change using classical plasticity [J]. Int. J. Plast., 2019, 119: 331
doi: 10.1016/j.ijplas.2019.04.006
|
| [72] |
Choi H, Yoon J W. A new simplified distortional hardening model for nonlinear strain paths [J]. Int. J. Plast., 2023, 165: 103617
doi: 10.1016/j.ijplas.2023.103617
|
| [73] |
Zhang H M, Xu S, Li Q, et al. Progress of crystal plasticity theory and simulations [J]. J. Plast. Eng., 2020, 27(5): 12
|
| [73] |
章海明, 徐 帅, 李 倩 等. 晶体塑性理论及模拟研究进展 [J]. 塑性工程学报, 2020, 27(5): 12
doi: 10.3969/j.issn.1007-2012.2020.05.003
|
| [74] |
Zecevic M, Korkolis Y P, Kuwabara T, et al. Dual-phase steel sheets under cyclic tension-compression to large strains: Experiments and crystal plasticity modeling [J]. J. Mech. Phys. Solids, 2016, 96: 65
doi: 10.1016/j.jmps.2016.07.003
|
| [75] |
Kim H, Barlat F, Lee Y, et al. A crystal plasticity model for describing the anisotropic hardening behavior of steel sheets during strain-path changes [J]. Int. J. Plast., 2018, 111: 85
doi: 10.1016/j.ijplas.2018.07.010
|
| [76] |
Xu Z T, Zhang R, Peng L F, et al. Crystal plasticity-based analysis and modelling of grain size and strain path dependent micro-scaled deformation mechanisms of ultra-thin sheet metals [J]. Int. J. Plast., 2023, 168: 103696
doi: 10.1016/j.ijplas.2023.103696
|
| [77] |
Iftikhar C M A, Li Y L, Kohar C P, et al. Evolution of subsequent yield surfaces with plastic deformation along proportional and non-proportional loading paths on annealed AA6061 alloy: Experiments and crystal plasticity finite element modeling [J]. Int. J. Plast., 2021, 143: 102956
doi: 10.1016/j.ijplas.2021.102956
|
| [78] |
Zhou C, Deng J J, Zhang W T, et al. A mixed hardening model for TRIP steel considering strain path change [J]. J. Plast. Eng., 2018, 25(4): 129
doi: 10.3969/j.issn.1007-2012.2018.04.019
|
| [78] |
周 驰, 邓军杰, 张文涛 等. 一种考虑应变路径变化的TRIP钢组合硬化模型 [J]. 塑性工程学报, 2018, 25(4): 129
|
| [79] |
Li J Z, Guan Z P, Chen J R, et al. A long short-term memory-based constitutive modeling framework for capturing strain path dependence in plastic deformation [J]. Mech. Mater., 2025, 205: 105325
doi: 10.1016/j.mechmat.2025.105325
|
| [80] |
Morand L, Helm D. A mixture of experts approach to handle ambiguities in parameter identification problems in material modeling [J]. Comput. Mater. Sci., 2019, 167: 85
doi: 10.1016/j.commatsci.2019.04.003
|
| [81] |
Gorji M B, Mozaffar M, Heidenreich J N, et al. On the potential of recurrent neural networks for modeling path dependent plasticity [J]. J. Mech. Phys. Solids, 2020, 143: 103972
doi: 10.1016/j.jmps.2020.103972
|
| [82] |
Zhang A N, Mohr D. Using neural networks to represent von Mises plasticity with isotropic hardening [J]. Int. J. Plast., 2020, 132: 102732
doi: 10.1016/j.ijplas.2020.102732
|
| [83] |
Jang D P, Fazily P, Yoon J W. Machine learning-based constitutive model for J2- plasticity [J]. Int. J. Plast., 2021, 138: 102919
doi: 10.1016/j.ijplas.2020.102919
|
| [84] |
Gu B, He J, Li S H, et al. Research progress on anisotropic fracture models and fracture tests for sheet metals [J]. J. Plast. Eng., 2019, 26(1): 1
doi: 10.3969/j.issn.1007-2012.2019.01.001
|
| [84] |
顾 彬, 何 霁, 李淑慧 等. 金属板料各向异性断裂模型及断裂实验研究进展 [J]. 塑性工程学报, 2019, 26(1): 1
|
| [85] |
Yoshida K, Kuwabara T, Kuroda M. Path-dependence of the forming limit stresses in a sheet metal [J]. Int. J. Plast., 2007, 23: 361
doi: 10.1016/j.ijplas.2006.05.005
|
| [86] |
Nurcheshmeh M, Green D E. Prediction of sheet forming limits with Marciniak and Kuczynski analysis using combined isotropic-nonlinear kinematic hardening [J]. Int. J. Mech. Sci., 2011, 53: 145
doi: 10.1016/j.ijmecsci.2010.12.004
|
| [87] |
Fincato R, Tsutsumi S, Momii H, et al. Ductile damage evolution under cyclic non-proportional loading paths [J]. Procedia Struct. Integr., 2018, 9: 136
doi: 10.1016/j.prostr.2018.06.022
|
| [88] |
Fan R L, Chen M H, Wu D P, et al. Prediction of damage and hot forming limit of TA32 titanium alloy based on crystal plasticity model [J]. Acta Metall. Sin., 2025, 61: 1293
doi: 10.11900/0412.1961.2023.00278
|
| [88] |
范荣磊, 陈明和, 吴迪鹏 等. 基于晶体塑性模型预测TA32钛合金损伤及高温成形极限 [J]. 金属学报, 2025, 61: 1293
doi: 10.11900/0412.1961.2023.00278
|
| [89] |
Nguyen N T, Tran M T, Nguyen X M, et al. Physics-guided machine learning for forming-limit assessments of advanced high-strength steels [J]. Int. J. Mech. Sci., 2025, 287: 109959
doi: 10.1016/j.ijmecsci.2025.109959
|
| [90] |
Pandya K S, Roth C C, Mohr D. Strain rate and temperature dependent fracture of aluminum alloy 7075: Experiments and neural network modeling [J]. Int. J. Plast., 2020, 135: 102788
doi: 10.1016/j.ijplas.2020.102788
|
| [91] |
Schowtjak A, Gerlach J, Muhammad W, et al. Prediction of ductile damage evolution based on experimental data using artificial neural networks [J]. Int. J. Solids Struct., 2022, 257: 111950
doi: 10.1016/j.ijsolstr.2022.111950
|
| [92] |
Qiao H, Guo X Q, Hong S G, et al. Modeling of {10-12}-{10-12} secondary twinning in pre-compressed Mg alloy AZ31 [J]. J. Alloys Compd., 2017, 725: 96
doi: 10.1016/j.jallcom.2017.07.133
|
| [93] |
Barrett T J, McCabe R J, Brown D W, et al. Predicting deformation behavior of α-uranium during tension, compression, load reversal, rolling, and sheet forming using elasto-plastic, multi-level crystal plasticity coupled with finite elements [J]. J. Mech. Phys. Solids, 2020, 138: 103924
doi: 10.1016/j.jmps.2020.103924
|
| [94] |
Upadhyay M V, Capek J, Panzner T, et al. Microstructure evolution of stainless steel subjected to biaxial load path changes: In-situ neutron diffraction and multi-scale modeling [J]. Int. J. Plast., 2019, 122: 49
doi: 10.1016/j.ijplas.2019.06.006
|
| [95] |
Kitayama K, Tomé C N, Rauch E F, et al. A crystallographic dislocation model for describing hardening of polycrystals during strain path changes. Application to low carbon steels [J]. Int. J. Plast., 2013, 46: 54
doi: 10.1016/j.ijplas.2012.09.004
|
| [96] |
Zhang Z, Shen F H, Münstermann S. Crystal plasticity modeling of prior austenite orientation effects on deformation behaviors of martensitic steels under different strain paths [J]. Mater. Des., 2024, 245: 113280
doi: 10.1016/j.matdes.2024.113280
|
| [97] |
Ibragimova O, Brahme A, Muhammad W, et al. A new ANN based crystal plasticity model for FCC materials and its application to non-monotonic strain paths [J]. Int. J. Plast., 2021, 144: 103059
doi: 10.1016/j.ijplas.2021.103059
|
| [98] |
Chen X F, Yu Z Q, Hou B, et al. A theoretical and experimental study on forming limit diagram for a seamed tube hydroforming [J]. J. Mater. Process. Technol., 2011, 211: 2012
doi: 10.1016/j.jmatprotec.2011.06.023
|
| [99] |
Dhara S, Basak S, Panda S K, et al. Formability analysis of pre-strained AA5754-O sheet metal using Yld96 plasticity theory: Role of amount and direction of uni-axial pre-strain [J]. J. Manuf. Process., 2016, 24: 270
doi: 10.1016/j.jmapro.2016.09.014
|
| [100] |
Leotoing L, Guines D. Investigations of the effect of strain path changes on forming limit curves using an in-plane biaxial tensile test [J]. Int. J. Mech. Sci., 2015, 99: 21
doi: 10.1016/j.ijmecsci.2015.05.007
|
| [101] |
Schlosser F, Signorelli J, Leonard M, et al. Influence of the strain path changes on the formability of a zinc sheet [J]. J. Mater. Process. Technol., 2019, 271: 101
doi: 10.1016/j.jmatprotec.2019.03.026
|
| [102] |
Guo J, Zhan M, Yang H. Advances in rolling-spinning technique of titanium tubes [J]. Mater. China, 2016, 35: 275
|
| [102] |
郭 靖, 詹 梅, 杨 合. 钛合金筒形件轧-旋成形研究进展 [J]. 中国材料进展, 2016, 35: 275
|
| [103] |
Wang X X, Zhan M, Gao P F, et al. Micromechanical behaviour of TA15 alloy cylindrical parts processed by multi-pass flow forming [J]. Mater. Sci. Eng., 2018, A737: 328
|
| [104] |
Yang B, Zhang W G, Lin Z Q. A method to design the loading path for tube hydroforming process [J]. J. Shanghai Jiao Tong Univ., 2006, 40: 893
|
| [104] |
杨 兵, 张卫刚, 林忠钦. 一种管件液压成形加载路径的设计方法 [J]. 上海交通大学学报, 2006, 40: 893
|
| [105] |
Teng B G, Li K, Yuan S J. Optimization of loading path in hydroforming T-shape using fuzzy control algorithm [J]. Int. J. Adv. Manuf. Technol., 2013, 69: 1079
doi: 10.1007/s00170-013-5086-7
|
| [106] |
Imaninejad M, Subhash G, Loukus A. Loading path optimization of tube hydroforming process [J]. Int. J. Mach. Tools Manuf., 2005, 45: 1504
doi: 10.1016/j.ijmachtools.2005.01.029
|
| [107] |
Zhang C, Liu W, Huang L R, et al. Process analysis of biconvex tube hydroforming based on loading path optimization by response surface method [J]. Int. J. Adv. Manuf. Technol., 2021, 112: 2609
doi: 10.1007/s00170-020-06411-6
|
| [108] |
Salandari-Rabori A, Zarei-Hanzaki A, Fatemi S M, et al. Microstructure and superior mechanical properties of a multi-axially forged WE magnesium alloy [J]. J. Alloys Compd., 2017, 693: 406
doi: 10.1016/j.jallcom.2016.09.198
|
| [109] |
Wang L. Study on the high-performance forming mechanism of TB6 titanium alloy shaped charge liner through controllable strain path forging [D]. Xi'an: Northwestern Polytechnical University, 2024
|
| [109] |
王 俐. TB6钛合金药型罩可控应变路径锻造高性能成形机理研究 [D]. 西安: 西北工业大学, 2024
|
| [110] |
Fan X G, Wang L, Jiang X Q, et al. Method for pre-treating and matching reversing large deformation refined titanium alloy microstructure [P]. Chin Pat, 202210099026.0, 2022
|
| [110] |
樊晓光, 王 俐, 姜雪琦 等. 一种预处理匹配换向大变形细化钛合金微观组织的方法 [P]. 中国专利, 202210099026.0, 2022)
|
| [111] |
Chen X H, Yu Z Q, Chen W, et al. Study on generating rolling method for manufacturing cylindrical parts with external cross ribs [J]. J. Manuf. Process., 2024, 111: 1
doi: 10.1016/j.jmapro.2024.01.009
|
| [112] |
Gao L Y, Fan Q B, Xu S, et al. Comparative investigation of deformation mechanisms in Ti-6Mo-3.5Cr-1Zr metastable β titanium alloy subject to cold rolling strain paths [J]. Mater. Sci. Eng., 2025, A941: 148661
|
| [113] |
Li W Y, Chen Z Y, Liu J R, et al. Rolling texture and its effect on tensile property of a near-α titanium alloy Ti60 plate [J]. J. Mater. Sci. Technol., 2019, 35: 790
doi: 10.1016/j.jmst.2018.10.032
|
| [114] |
Rouzbeh A, Sedighi M, Hashemi R. Effects of strain path on the microstructure, tensile properties, and formability of Al/Mg roll-bonded sheets [J]. J. Mater. Res. Technol., 2023, 23: 5318
doi: 10.1016/j.jmrt.2023.02.148
|
| [115] |
Zhang Z M, Li G J, Wang Q, et al. Multi-directional loading rotary extrusion forming technology and equipment [J]. J. Mech. Eng., 2023, 59(12): 264
doi: 10.3901/JME.2023.12.264
|
| [115] |
张治民, 李国俊, 王 强 等. 多向加载旋转挤压成形技术及装备 [J]. 机械工程学报, 2023, 59(12): 264
doi: 10.3901/JME.2023.12.264
|
| [116] |
Mills K, Li H J, Luzin V, et al. Influence of ECAP deformation routes on grain refinement, mechanical properties and texture of zinc [J]. Mater. Sci. Eng., 2025, A945: 149066
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
| |
Shared |
|
|
|
|
| |
Discussed |
|
|
|
|