| 金属材料在高温高压水、液态Pb-Bi和海洋环境中的腐蚀疲劳行为研究进展 |
吴欣强( ), 谭季波, 张兹瑜, 薛宝权, 柯伟 |
| 中国科学院金属研究所 中国科学院核用材料与安全评价重点实验室 沈阳 110016 |
|
| Research Advance on Corrosion Fatigue Behavior of Metallic Materials in High-Temperature Pressurized Water, Liquid Pb-Bi, and Marine Environments |
WU Xinqiang( ), TAN Jibo, ZHANG Ziyu, XUE Baoquan, KE Wei |
| CAS Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China |
引用本文:
吴欣强, 谭季波, 张兹瑜, 薛宝权, 柯伟. 金属材料在高温高压水、液态Pb-Bi和海洋环境中的腐蚀疲劳行为研究进展[J]. 金属学报, 2026, 62(5): 822-834.
Xinqiang WU,
Jibo TAN,
Ziyu ZHANG,
Baoquan XUE,
Wei KE.
Research Advance on Corrosion Fatigue Behavior of Metallic Materials in High-Temperature Pressurized Water, Liquid Pb-Bi, and Marine Environments[J]. Acta Metall Sin, 2026, 62(5): 822-834.
| [1] |
Ma Y J, Zhang Z Y, Tan J B, et al. Microstructurally and mechanically small fatigue crack growth behaviors of 316LN stainless steel in high-temperature pressurized water [J]. Corros. Sci., 2024, 227: 111735
doi: 10.1016/j.corsci.2023.111735
|
| [2] |
Ma Y J, Zhang Z Y, Zhang X, et al. Effects of strain rate on low-cycle fatigue crack growth behavior of 316LN weld metal in high-temperature pressurized water [J]. Corros. Sci., 2022, 199: 110169
doi: 10.1016/j.corsci.2022.110169
|
| [3] |
Ma Y J, Zhang Z Y, Tan J B, et al. Effect of surface roughness on low-cycle fatigue behaviors of 316LN stainless steel in borated and lithiated high-temperature pressurized water [J]. Corros. Sci., 2022, 209: 110792
doi: 10.1016/j.corsci.2022.110792
|
| [4] |
Gao J, Zhang Z Y, Tan J B, et al. Differences of corrosion fatigue behaviors among 316LN base metal, 316LN heat-affected zone and 308L weld metal in a safe-end weld joint in borated and lithiated high-temperature water [J]. Int. J. Fatigue, 2021, 148: 106223
doi: 10.1016/j.ijfatigue.2021.106223
|
| [5] |
Gao J, Tan J B, Zhang Z Y, et al. Effects of welding columnar grain orientation and strain rate on corrosion fatigue behavior of alloy 52/52M weld metal in high-temperature water [J]. Corros. Sci., 2021, 180: 109196
doi: 10.1016/j.corsci.2020.109196
|
| [6] |
Gao J, Zhang Z Y, Tan J B, et al. Environmentally assisted fatigue behavior of 308L weld metal in borated and lithiated high-temperature water [J]. J. Nucl. Mater., 2020, 539: 152365
doi: 10.1016/j.jnucmat.2020.152365
|
| [7] |
Gao J, Tan J B, Wu X Q, et al. Effect of grain boundary engineering on corrosion fatigue behavior of 316LN stainless steel in borated and lithiated high-temperature water [J]. Corros. Sci., 2019, 152: 190
doi: 10.1016/j.corsci.2019.01.036
|
| [8] |
Gao J, Tan J B, Jiao M, et al. Role of welding residual strain and ductility dip cracking on corrosion fatigue behavior of alloy 52/52M dissimilar metal weld in borated and lithiated high-temperature water [J]. J. Mater. Sci. Technol., 2020, 42: 163
doi: 10.1016/j.jmst.2019.10.012
|
| [9] |
Tan J B, Zhang Z Y, Zheng H, et al. Corrosion fatigue model of austenitic stainless steels used in pressurized water reactor nuclear power plants [J]. J. Nucl. Mater., 2020, 541: 152407
doi: 10.1016/j.jnucmat.2020.152407
|
| [10] |
Tan J B, Wu X Q, Han E H, et al. Strain-rate dependent fatigue behavior of 316LN stainless steel in high-temperature water [J]. J. Nucl. Mater., 2017, 489: 33
doi: 10.1016/j.jnucmat.2017.03.040
|
| [11] |
Tan J B, Wu X Q, Han E H, et al. The effect of dissolved oxygen on fatigue behavior of alloy 690 steam generator tubes in borated and lithiated high temperature water [J]. Corros. Sci., 2016, 102: 394
doi: 10.1016/j.corsci.2015.10.032
|
| [12] |
Tan J B, Wu X Q, Han E H, et al. Role of TiN inclusion on corrosion fatigue behavior of alloy 690 steam generator tubes in borated and lithiated high temperature water [J]. Corros. Sci., 2014, 88: 349
doi: 10.1016/j.corsci.2014.07.059
|
| [13] |
Tan J B, Wu X Q, Han E H, et al. Corrosion fatigue behavior of alloy 690 steam generator tube in borated and lithiated high temperature water [J]. Corros. Sci., 2014, 89: 203
doi: 10.1016/j.corsci.2014.08.027
|
| [14] |
Zhang Z Y, Tan J B, Wu X Q, et al. Corrosion fatigue crack growth behavior of 316LN stainless steel in high-temperature pressurized water [J]. Nucl. Eng. Technol., 2021, 53: 2977
doi: 10.1016/j.net.2021.03.016
|
| [15] |
Zhang Z Y, Tan J B, Wu X Q, et al. Corrosion fatigue behavior and crack-tip characteristic of 316LN stainless steel in high-temperature pressurized water [J]. J. Nucl. Mater., 2019, 518: 21
doi: 10.1016/j.jnucmat.2019.02.040
|
| [16] |
Zhang Z Y, Tan J B, Wu X Q, et al. Effects of temperature on corrosion fatigue behavior of 316LN stainless steel in high-temperature pressurized water [J]. Corros. Sci., 2019, 146: 80
doi: 10.1016/j.corsci.2018.10.023
|
| [17] |
Zhang Z Y, Tan J B, Wu X Q, et al. Synergistic effect of mechanical and environmental damages of 316LN stainless steel under different fatigue strain amplitudes in high-temperature pressurized water [J]. Mater. Sci. Eng., 2019, A743: 243
|
| [18] |
Xue B Q, Tan J B, Wu X Q, et al. Unveiling liquid Pb-Bi embrittlement of 316LN stainless steel under fatigue crack propagation tests through multiscale advanced characterization [J]. Corros. Sci., 2025, 246: 112752
doi: 10.1016/j.corsci.2025.112752
|
| [19] |
Xue B Q, Wang W, Tan J B, et al. Insights into the fatigue damage mechanism of T91 steel in liquid lead-bismuth eutectic at 150-550 oC [J]. Corros. Sci., 2024, 232: 112007
doi: 10.1016/j.corsci.2024.112007
|
| [20] |
Xue B Q, Tan J B, Wu X Q, et al. Strain-rate dependent fatigue behavior of T91 steel at 550 °C of liquid lead-bismuth eutectic [J]. Corros. Sci., 2024, 240: 112433
doi: 10.1016/j.corsci.2024.112433
|
| [21] |
Xue B Q, Tan J B, Wu X Q, et al. Insights into fatigue crack propagation mechanism of T91 steel in liquid lead-bismuth eutectic at 150-450 oC [J]. Corros. Sci., 2024, 236: 112264
doi: 10.1016/j.corsci.2024.112264
|
| [22] |
Xue B Q, Tan J B, Zhang Z Y, et al. Effect of temperature on low cycle fatigue behavior of T91 steel in liquid lead-bismuth eutectic environment at 150-550 oC [J]. Int. J. Fatigue, 2023, 167: 107344
doi: 10.1016/j.ijfatigue.2022.107344
|
| [23] |
Xue B Q, Tan J B, Wu X Q, et al. A novel monitoring system for fatigue crack length of compact tensile specimen in liquid lead-bismuth eutectic [J]. Nucl. Eng. Technol., 2024, 56: 1887
doi: 10.1016/j.net.2023.12.051
|
| [24] |
ASTM. ASTM E466-21 Standard practice for conducting force controlled constant amplitude axial fatigue tests of metallic materials [S]. West Conshohocken: ASTM, 2021
|
| [25] |
ASTM. ASTM E606/E606M-21 Standard test method for strain-controlled fatigue testing[S]. West Conshohocken: ASTM, 2021
|
| [26] |
ASTM. ASTM E2714-13 Standard test method for creep-fatigue testing [S]. West Conshohocken: ASTM, 2020
|
| [27] |
ASTM. ASTM E647-08 Standard test method for measurement of fatigue crack growth rates [S]. West Conshohocken: ASTM, 2008
|
| [28] |
Riccioli F, Alkhateeb S, Mol A, et al. Feasibility assessment of non-contact acoustic emission monitoring of corrosion-fatigue damage in submerged steel structures [J]. Ocean Eng., 2024, 312: 119296
doi: 10.1016/j.oceaneng.2024.119296
|
| [29] |
Tan J B, Zhang Q, Wang X, et al. Fatigue test device in high-temperature liquid lead bismuth environment [P]. Chin Pat, 202120775649.6, 2021
|
| [29] |
谭季波, 张 强, 王 翔 等. 一种高温液态铅铋环境中的疲劳试验装置 [P]. 中国专利, 202120775649.6, 2021
|
| [30] |
Evans C, Leiva-Garcia R, Akid R. Strain evolution around corrosion pits under fatigue loading [J]. Theor. Appl. Fract. Mech., 2018, 95: 253
doi: 10.1016/j.tafmec.2018.02.015
|
| [31] |
Okenyi V, Afazov S, Mansfield N, et al. Corrosion surface morphology-based methodology for fatigue assessment of offshore welded structures [J]. Fatigue Fract. Eng. Mater. Struct., 2023, 46: 4663
doi: 10.1111/ffe.v46.12
|
| [32] |
Gabb T P, Telesman J, Hazel B, et al. The effects of hot corrosion pits on the fatigue resistance of a disk superalloy [J]. J. Mater. Eng. Perform., 2010, 19: 77
doi: 10.1007/s11665-009-9399-5
|
| [33] |
Li Y, Guan L, Wang G, et al. Influence of mechanical stresses on pitting corrosion of stainless steel [J]. J. Chin. Soc. Corros. Prot., 2019, 39: 215
|
| [33] |
李 雨, 关 蕾, 王 冠 等. 机械应力对不锈钢点蚀行为的影响 [J]. 中国腐蚀与防护学报, 2019, 39: 215
|
| [34] |
Rimkevicius S, Kaliatka A, Valincius M, et al. Development of approach for reliability assessment of pipeline network systems [J]. Appl. Energy, 2012, 94: 22
doi: 10.1016/j.apenergy.2012.01.015
|
| [35] |
Ebara R. Corrosion fatigue crack initiation behavior of stainless steels [J]. Procedia Eng., 2010, 2: 1297
doi: 10.1016/j.proeng.2010.03.141
|
| [36] |
Frankel G S. Pitting corrosion of metals: A review of the critical factors [J]. J. Electrochem. Soc., 1998, 145: 2186
doi: 10.1149/1.1838615
|
| [37] |
Adedipe O, Brennan F, Mehmanparast A, et al. Corrosion fatigue crack growth mechanisms in offshore monopile steel weldments [J]. Fatigue Fract. Eng. Mater. Struct., 2017, 40: 1868
doi: 10.1111/ffe.v40.11
|
| [38] |
Laleh M, Huo Y, Kannan M B, et al. Probing and monitoring multiple forms of localised corrosion occurring concurrently on pipeline steels in marine environments [J]. Corros. Sci., 2024, 240: 112453
doi: 10.1016/j.corsci.2024.112453
|
| [39] |
Choudhary S, Kelly R G, Birbilis N. On the origin of passive film breakdown and metastable pitting for stainless steel 316L [J]. Corros. Sci., 2024, 230: 111911
doi: 10.1016/j.corsci.2024.111911
|
| [40] |
Chen S, Sun L, Cao W K, et al. Research on the pitting behavior of high nitrogen austenitic stainless steel 316LN in sodium chloride solution by using modified potentiostatic pulse test [J]. J. Electroanal. Chem., 2022, 922: 116739
doi: 10.1016/j.jelechem.2022.116739
|
| [41] |
Duan Z W, Man C, Dong C F, et al. Pitting behavior of SLM 316L stainless steel exposed to chloride environments with different aggressiveness: Pitting mechanism induced by gas pores [J]. Corros. Sci., 2020, 167: 108520
doi: 10.1016/j.corsci.2020.108520
|
| [42] |
Ehrnstén U, Andresen P L, Que Z Q. A review of stress corrosion cracking of austenitic stainless steels in PWR primary water [J]. J. Nucl. Mater., 2024, 588: 154815
doi: 10.1016/j.jnucmat.2023.154815
|
| [43] |
Hong S, Min K D, Jeon S H, et al. Environmental fatigue crack growth rate of type 347 austenitic stainless steel in simulated PWR water conditions [J]. Int. J. Press. Vessels Pip., 2018, 167: 11
doi: 10.1016/j.ijpvp.2018.10.003
|
| [44] |
Seifert H P, Ritter S, Leber H J. Corrosion fatigue crack growth behaviour of austenitic stainless steels under light water reactor conditions [J]. Corros. Sci., 2012, 55: 61
doi: 10.1016/j.corsci.2011.10.005
|
| [45] |
Ruther W E, Soppett W K, Kassner T F. Corrosion fatigue of alloys 600 and 690 in simulated LWR environments [R]. Washington: U.S. Nuclear Regulatory Commission, 1996
|
| [46] |
Li S P, Dang Y, Hong X F, et al. Effect of water chemistry on corrosion behavior of nickel-based alloy 690 in high temperature high pressure water [J]. J. Chin. Soc. Corros. Prot., 2025, 45: 1035
|
| [46] |
李顺平, 党 莹, 洪晓峰 等. 水化学对690镍基合金高温高压水腐蚀行为的影响 [J]. 中国腐蚀与防护学报, 2025, 45: 1035
doi: 10.11902/1005.4537.2024.414
|
| [47] |
Fruzzetti K, Ahluwalia K, Hickling J. Materials reliability program: Effects of hydrogen, pH, lithium and boron on primary water stress corrosion crack initiation in alloy 600 for temperatures in the range 320-330 oC (MRP-147) [R]. Palo Alto: Electric Power Research Institute, 2005
|
| [48] |
Liu R, Liu L, Wang F H. The role of hydrostatic pressure on the metal corrosion in simulated deep-sea environments—A review [J]. J. Mater. Sci. Technol., 2022, 112: 230
doi: 10.1016/j.jmst.2021.10.014
|
| [49] |
Duan T G, Peng W S, Ding K K, et al. Long-term field exposure corrosion behavior investigation of 316L stainless steel in the deep sea environment [J]. Ocean Eng., 2019, 189: 106405
doi: 10.1016/j.oceaneng.2019.106405
|
| [50] |
Li Y, Zhao Y Y, Deng C Y, et al. Analysis of fatigue crack growth rate of welded joint after immersion corrosion [J]. Trans. China Weld. Inst., 2024, 45(9): 14
|
| [50] |
李 岳, 赵洋洋, 邓彩艳 等. 全浸腐蚀后焊接接头疲劳裂纹扩展速率分析 [J]. 焊接学报, 2024, 45(9): 14
|
| [51] |
Liu H C, Fan L, Zhang H B, et al. Research progress of stress corrosion cracking of Ti-alloy in deep sea environments [J]. J. Chin. Soc. Corros. Prot., 2022, 42: 175
|
| [51] |
柳皓晨, 范 林, 张海兵 等. 钛合金深海应力腐蚀研究进展 [J]. 中国腐蚀与防护学报, 2022, 42: 175
doi: 10.11902/1005.4537.2021.050
|
| [52] |
Alqahtani I, Starr A, Khan M. Fracture behaviour of aluminium alloys under coastal environmental conditions: A review [J]. Metals, 2024, 14: 336
doi: 10.3390/met14030336
|
| [53] |
Cao A G, Zong H, Liu X X, et al. Application of 15-5PH stainless steel fasteners in high seawater salt fog environment [J]. Corros. Prot., 2024, 45(7): 84
|
| [53] |
曹安港, 宗 浩, 刘欣欣 等. 15-5PH不锈钢紧固件在高海水盐雾环境中的应用 [J]. 腐蚀与防护, 2024, 45(7): 84
|
| [54] |
Zhou X F, Lv X Y, Wu S J, et al. Corrosion fatigue properties of hot continuous rolling Ti-Al-Nb-Zr-Mo alloy seamless tube by electron beam welding in 3.5% NaCl solution [J]. J. Mater. Eng. Perform., 2025, 34: 5063
doi: 10.1007/s11665-024-09466-8
|
| [55] |
Fan Y, Su H Z, Chen K, et al. Corrosion fatigue crack growth behavior of austenitic stainless steels in seawater environment [J]. Corros. Prot., 2020, 41(7): 67
|
| [55] |
范 镒, 苏豪展, 陈 凯 等. 奥氏体不锈钢在海水环境中的腐蚀疲劳裂纹扩展行为 [J]. 腐蚀与防护, 2020, 41(7): 67
|
| [56] |
Zhao Y X, Yu P S, Wu L S, et al. Corrosion-induced deceleration-to-acceleration of fatigue crack growth for deep-sea Ti6Al4V ELI titanium alloy [J]. Eng. Fract. Mech., 2023, 281: 109160
doi: 10.1016/j.engfracmech.2023.109160
|
| [57] |
Yu C L, Guo Q B, Gong X B, et al. Fatigue life assessment of pressure hull of deep-sea submergence vehicle [J]. Ocean Eng., 2022, 245: 110528
doi: 10.1016/j.oceaneng.2022.110528
|
| [58] |
Wang L, Ye C, Sun C Q, et al. Experimental investigation on compressive dwell fatigue behavior of titanium alloy pressure hull for deep-sea manned submersibles [J]. Ocean Eng., 2024, 303: 117646
doi: 10.1016/j.oceaneng.2024.117646
|
| [59] |
Sun C Q, Li Y Q, Xu K L, et al. Effects of intermittent loading time and stress ratio on dwell fatigue behavior of titanium alloy Ti-6Al-4V ELI used in deep-sea submersibles [J]. J. Mater. Sci. Technol., 2021, 77: 223
doi: 10.1016/j.jmst.2020.10.063
|
| [60] |
Jin Y, Liu R, Cui Y, et al. Study on corrosion fatigue of Ti-6Al-4V alloy under hydrostatic pressure environment in 3.5 % NaCl solution [J]. Corros. Sci., 2025, 252: 112950
doi: 10.1016/j.corsci.2025.112950
|
| [61] |
Wu Y M, Zhao W J, Wang L P. State of the art and current trends on the metal corrosion and protection strategies in deep sea [J]. J. Mater. Sci. Technol., 2025, 215: 192
doi: 10.1016/j.jmst.2024.07.026
|
| [62] |
Ren P W, Meng H M, Xia Q J, et al. Tribocorrosion of 316L stainless steel by in-situ electrochemical methods under deep-sea high hydrostatic pressure environment [J]. Corros. Sci., 2022, 202: 110315
doi: 10.1016/j.corsci.2022.110315
|
| [63] |
Traverso P, Canepa E. A review of studies on corrosion of metals and alloys in deep-sea environment [J]. Ocean Eng., 2014, 87: 10
doi: 10.1016/j.oceaneng.2014.05.003
|
| [64] |
Liu J G, Guo Y G, Xing X, et al. A comprehensive review on hydrogen permeation barrier in the hydrogen transportation pipeline: Mechanism, application, preparation, and recent advances [J]. Int. J. Hydrogen Energy, 2025, 101: 504
doi: 10.1016/j.ijhydene.2024.12.379
|
| [65] |
Barrera O, Bombac D, Chen Y, et al. Understanding and mitigating hydrogen embrittlement of steels: A review of experimental, modelling and design progress from atomistic to continuum [J]. J. Mater. Sci., 2018, 53: 6251
doi: 10.1007/s10853-017-1978-5
pmid: 31258179
|
| [66] |
Birnbaum H K, Sofronis P. Hydrogen-enhanced localized plasticity—A mechanism for hydrogen-related fracture [J]. Mater. Sci. Eng., 1994, A176: 191
|
| [67] |
Hoang P H, Gangadharan A, Ramalingam S C. Primary water stress corrosion cracking inspection ranking scheme for alloy 600 components [J]. Nucl. Eng. Des., 1998, 181: 209
doi: 10.1016/S0029-5493(97)00346-4
|
| [68] |
Rebak R B, Szklarska-smialowska Z. The mechanism of stress corrosion cracking of alloy 600 in high temperature water [J]. Corros. Sci., 1996, 38: 971
doi: 10.1016/0010-938X(96)00183-7
|
| [69] |
Li Y, Liu Z Y, Fan E D, et al. The effect of crack tip environment on crack growth behaviour of a low alloy steel at cathodic potentials in artificial seawater [J]. J. Mater. Sci. Technol., 2020, 54: 119
doi: 10.1016/j.jmst.2020.04.034
|
| [70] |
Li Z, Fan L, Ma L, et al. Perspective review on factors that influence the stress corrosion of Ti alloys for deep-sea applications [J]. J. Mater. Sci. Technol., 2025, 222: 228
doi: 10.1016/j.jmst.2024.10.022
|
| [71] |
Komoda R, Kubota M, Staykov A, et al. Effect of water temperature in the deep sea on the mitigation of hydrogen embrittlement by O2 impurity [J]. Eng. Fail. Anal., 2025, 180: 109885
doi: 10.1016/j.engfailanal.2025.109885
|
| [72] |
Li Y, Zhou X K, Dou Y N, et al. Numerical analysis of dynamic and fatigue characteristics of deep-sea mining riser considering irregular waves and currents [J]. Ocean Eng., 2024, 311: 118910
doi: 10.1016/j.oceaneng.2024.118910
|
| [73] |
Guo Y H, Wang S C, Liu G. Creep-fatigue life prediction of a titanium alloy deep-sea submersible using a continuum damage mechanics-informed BP neural network model [J]. Ocean Eng., 2024, 311: 118826
doi: 10.1016/j.oceaneng.2024.118826
|
| [74] |
Guo Y H, Liu G, Xu J C, et al. Numerical analysis on the creep-fatigue damage of titanium alloy deep-sea pressure hull at room temperature [J]. Mar. Struct., 2024, 96: 103639
doi: 10.1016/j.marstruc.2024.103639
|
| [75] |
Zhang T M, Zhao W M, Li T T, et al. Comparison of hydrogen embrittlement susceptibility of three cathodic protected subsea pipeline steels from a point of view of hydrogen permeation [J]. Corros. Sci., 2018, 131: 104
doi: 10.1016/j.corsci.2017.11.013
|
| [76] |
Wan H X, Du C W, Liu Z Y, et al. The effect of hydrogen on stress corrosion behavior of X65 steel welded joint in simulated deep sea environment [J]. Ocean Eng., 2016, 114: 216
doi: 10.1016/j.oceaneng.2016.01.020
|
| [77] |
Rostoker W, McCaughey J M, Markus H. Embrittlement by Liquid Metals [M]. New York: Reinhold Publishing Corporation, 1960: 1
|
| [78] |
Gong X, Short M P, Auger T, et al. Environmental degradation of structural materials in liquid lead- and lead-bismuth eutectic-cooled reactors [J]. Prog. Mater. Sci., 2022, 126: 100920
doi: 10.1016/j.pmatsci.2022.100920
|
| [79] |
Basquin O H. The exponential law of endurance tests [A]. Proceedings of the 10th Annual Meeting [C]. Atlantic City: ASTM, 1910: 625
|
| [80] |
Coffin L F. A study of the effects of cyclic thermal stresses on a ductile metal [J]. J. Fluids Eng., 1954, 76: 931
|
| [81] |
Manson S S. Behavior of materials under conditions of thermal stress [R]. Washington: National Advisory Committee for Aeronautics, 1953
|
| [82] |
Miner M A. Cumulative damage in fatigue [J]. J. Appl. Mech., 1945, 12: A159
doi: 10.1115/1.4009458
|
| [83] |
Langer B F. Design of pressure vessels for low-cycle fatigue [J]. J. Basic Eng., 1962, 84: 389
doi: 10.1115/1.3657332
|
| [84] |
Wu X Q, Rong L J, Tan J B, et al. Research advance on liquid lead-bismuth eutectic corrosion resistant Si enhanced ferritic/martensitic and austenitic stainless steels [J]. Acta Metall. Sin., 2023, 59: 502
doi: 10.11900/0412.1961.2022.00531
|
| [84] |
吴欣强, 戎利建, 谭季波 等. 耐Pb-Bi腐蚀Si增强型铁素体/马氏体钢和奥氏体不锈钢的研究进展 [J]. 金属学报, 2023, 59: 502
doi: 10.11900/0412.1961.2022.00531
|
| [85] |
Chopra O K, Stevens G L. Effect of LWR coolant environments on the fatigue life of reactor materials [R]. Washington: U.S. Nuclear Regulatory Commission, 2018
|
| [86] |
Japan Nuclear Energy Safety Organization. Environmental fatigue evaluation method for nuclear power plants [R]. Tokyo: Japan Nuclear Energy Safety, 2011
|
| [87] |
Godard H P. The corrosion behavior of aluminum in natural waters [J]. Can. J. Chem. Eng., 1960, 38: 167
doi: 10.1002/cjce.v38:5
|
| [88] |
Harlow D G, Wei R P. Probability approach for prediction of corrosion and corrosion fatigue life [J]. AIAA J., 1994, 32: 2073
doi: 10.2514/3.12254
|
| [89] |
Sriraman M R, Pidaparti R M. Life prediction of aircraft aluminum subjected to pitting corrosion under fatigue conditions [J]. J. Aircr., 2009, 46: 1253
doi: 10.2514/1.40481
|
| [90] |
Li S X, Akid R. Corrosion fatigue life prediction of a steel shaft material in seawater [J]. Eng. Fail. Anal., 2013, 34: 324
doi: 10.1016/j.engfailanal.2013.08.004
|
| [91] |
Paris P, Erdogan F. A critical analysis of crack propagation laws [J]. J. Fluids Eng., 1963, 85: 528
|
| [92] |
ASME. N-809 Reference fatigue crack growth rate curves for austenitic stainless steels in pressurized reactor water environments [S]. New York: ASME, 2015
|
| [93] |
Chan K S, Enright M P, Moody J, et al. A microstructure-based time-dependent crack growth model for life and reliability prediction of turbopropulsion systems [J]. Metall. Mater. Trans., 2014, 45A: 287
|
| [94] |
Pressouyre G M, Bernstein I M. A quantitative analysis of hydrogen trapping [J]. Metall. Trans., 1978, 9A: 1571
|
| [95] |
Turnbull A, de Maria M S S. Predicting the kinetics of hydrogen generation at the tips of corrosion fatigue cracks [J]. Metall. Trans., 1988, 19A: 1795
|
| [96] |
Masuda H, Nishijima S. Application of scratching electrode method for corrosion fatigue [J]. Corros. Eng., 1985, 34: 30
doi: 10.3323/jcorr1974.34.1_30
|
| [97] |
Zhao Y X, Wang J N, Gao Q. A unified classical maximum likelihood approach for estimating P-S-N curves of three commonly used fatigue stress-life relations [J]. Chin. J. Appl. Mech., 2001, 18(1): 83
|
| [97] |
赵永翔, 王金诺, 高 庆. 估计三种常用疲劳应力-寿命模型P-S-N曲线的统一经典极大似然法 [J]. 应用力学学报, 2001, 18(1): 83
|
| [98] |
Xu H H, Ao N, Wu S C, et al. Research progress on corrosion fatigue life prediction models of metal structural materials [J]. Chin. J. Solid Mech., 2023, 44: 1
|
| [98] |
徐会会, 奥 妮, 吴圣川 等. 金属结构材料腐蚀疲劳寿命预测模型的研究进展 [J]. 固体力学学报, 2023, 44: 1
|
| [99] |
Zhang T Y. An Introduction to Materials Informatics (I): The Elements of Machine Learning [M]. Beijing: Science Press, 2022: 1
|
| [99] |
张统一. 材料信息学导论(上): 机器学习基础 [M]. 北京: 科学出版社, 2022: 1
|
| [100] |
Bao H Y X, Wu S C, Wu Z K, et al. A machine-learning fatigue life prediction approach of additively manufactured metals [J]. Eng. Fract. Mech., 2021, 242: 107508
doi: 10.1016/j.engfracmech.2020.107508
|
| [101] |
Zhan Z X, Li H. Machine learning based fatigue life prediction with effects of additive manufacturing process parameters for printed SS 316L [J]. Int. J. Fatigue, 2021, 142: 105941
doi: 10.1016/j.ijfatigue.2020.105941
|
| [102] |
Haque M E, Sudhakar K V. Prediction of corrosion-fatigue behavior of DP steel through artificial neural network [J]. Int. J. Fatigue, 2001, 23: 1
|
| [103] |
Zhang X C, Gong J G, Xuan F Z. A physics-informed neural network for creep-fatigue life prediction of components at elevated temperatures [J]. Eng. Fract. Mech., 2021, 258: 108130
doi: 10.1016/j.engfracmech.2021.108130
|
| [104] |
Neerukatti R K, Liu K C, Kovvali N, et al. Fatigue life prediction using hybrid prognosis for structural health monitoring [J]. J. Aerosp. Inf. Syst., 2014, 11: 211
|
| [105] |
Yang Y F, Chen C H, Zhuang Y F, et al. Reviewing the progress of corrosion fatigue research on marine structures [J]. Front. Mater., 2024, 11: 1399292
doi: 10.3389/fmats.2024.1399292
|
| [106] |
Feng S W, Sun X Y, Chen G, et al. LBE corrosion fatigue life prediction of T91 steel and 316 SS using machine learning method assisted by symbol regression [J]. Int. J. Fatigue, 2023, 177: 107962
doi: 10.1016/j.ijfatigue.2023.107962
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
| |
Shared |
|
|
|
|
| |
Discussed |
|
|
|
|