Effect of Strain Rate on the Strain Partitioning Behavior of Ferrite/Bainite in X80 Pipeline Steel
WANG Nan1, CHEN Yongnan1(), ZHAO Qinyang1, WU Gang2, ZHANG Zhen1, LUO Jinheng2
1.School of Materials Science and Engineering, Chang'an University, Xi'an 710064, China 2.CNPC Tubular Goods Research Institute, Xi'an 710077, China
Cite this article:
WANG Nan, CHEN Yongnan, ZHAO Qinyang, WU Gang, ZHANG Zhen, LUO Jinheng. Effect of Strain Rate on the Strain Partitioning Behavior of Ferrite/Bainite in X80 Pipeline Steel. Acta Metall Sin, 2023, 59(10): 1299-1310.
X80 pipeline steel, which is mainly composed of ferrite/bainite, is an important structural steel for pipeline transportation. The plastic deformation of X80 pipeline steel at different strain rates caused by geological and human factors deteriorates its strength. Microstructural transformation and strain localization during deformation are the fundamental factors that deteriorate the mechanical properties of steel. Therefore, in this study, the strain partitioning behavior and microstructure evolution mechanism of ferrite and bainite in X80 pipeline steel at different strain rates (10-4 s-1 to 10-1 s-1) under 5% deformation were revealed using representative volume element models and electron backscatter diffraction technology. The results show that when the strain rate is low (10-4 s-1 to 10-3 s-1), ferrite has sufficient time to complete the evolution of geometrically necessary dislocations (GNDs) to low-angle grain boundaries (LAGBs) and the transformation of LAGBs to high-angle grain boundaries (HAGBs). Ferrite can release strain distortion energy, which can weaken the strain localization behavior of X80 steel. As the strain rate increases, the strain response time decreases, hindering the transition from LAGBs to HAGBs. This results in the accumulation of high-density GNDs and LAGBs in ferrite, thereby intensifying strain localization. Additionally, when the strain rate is high (10-2 s-1 to 10-1 s-1), the strain partitioning coefficient between ferrite and bainite could be reduced, thereby producing the strain gradient in the vicinity of the interface and resulting in GNDs accumulation and back stress formation. Furthermore, ferrite and bainite could show compressive and tensile stresses, respectively, thus limiting the strain coordination between the two phases significantly, increasing the stress concentration near the interface, and reducing the strain hardening ability. The strain partitioning behavior between ferrite and bainite was further revealed to better understand the plastic deformation of X80 pipeline steel.
Fig.1 Schematics of making representative volume element (RVE) model (a-e) and true stress-strain curves of ferrite and bainite (f) (a) OM image (b) locally magnified OM image (c) binarization model (d) boundary line model (e) boundary condition of displacement (Ux and U represent the displacement of x-axis and boundary displacement direction, respectively)
Phase
σy / MPa
εy
E / GPa
n
Ferrite
370
0.003
180
0.173
Bainite
830
0.005
190
0.102
Table 1 Mechanical property parameters of ferrite and bainite[21]
Fig.2 Equivalent plastic strain (PEEQ) distributions under deformation of 5% at strain rates of 10-4 s-1 (a1-a3), 10-3 s-1 (b1-b3), 10-2 s-1 (c1-c3), and 10-1 s-1 (d1-d3) for ferrite (a1-d1), bainite (a2-d2), and X80 steel (a3-d3)
Fig.3 Probability density functions at strain rates of 10-4 s-1 (a) and 10-1 s-1 (b), strain localization factor (c), cumulative density functions (CDF) at strain rates of 10-4 s-1 (d) and 10-1 s-1 (e), and plastic deformation difference between two phases (f) of ferrite and bainite under deformation of 5%
Fig.4 Strain partitioning behaviors between ferrite and bainite (a) true stress-strain curve at strain rate of 10-4 s-1 (b) strain partitioning coefficient
Fig.5 Engineering stress-strain curves (a) and strain rate sensitivity indexes (m) (b) under different strain rates
Strain rate / s-1
Yield stress / MPa
Tensile stress / MPa
Yield ratio
Uniform elongation / %
10-4
586
644
0.91
18.73
10-3
613
651
0.94
17.61
10-2
627
667
0.94
15.27
10-1
635
685
0.93
13.77
Table 2 Mechanical properties of X80 steel under different strain rates
Fig.6 Kernel average misorientation (KAM) maps of X80 steel after deformation of 5% at strain rates of 10-4 s-1 (a), 10-3 s-1 (b), 10-2 s-1 (c), and 10-1 s-1 (d) (Inset shows the strain gradient between ferrite and bainite)
Fig.7 Schematic of back stress caused by geometrically necessary dislocations (GNDs) accumulation (a) and GND densities after different strain rates (b)
Fig.8 Grain boundary distribution maps at strains rates of 10-4 s-1 (a) and 10-1 s-1 (b) (Black lines represent high-angle grain boundaries (HAGBs) and red lines represent low-angle grain boundaries (LAGBs)), and misorientation statistical diagrams at strain rates of 10-4 s-1 (c), 10-3 s-1 (d), 10-2 s-1 (e), and 10-1 s-1 (f) in X80 steel
Fig.9 Relative volume fractions of LAGBs and HAGBs under different strain rates
Fig.10 Schematic of the microstructure evolution for ferrite under low strain rate and high strain rate from yield to 5% deformation in X80 steel
Fig.11 Strain hardening behaviors of X80 steel under different strain rates (a) true stress-strain curves (b) modified C-J model (εI-II is the strain at the transition point from stage I to stage II, and εII-III is the strain at the transition point from stage II to stage III)
Strain rate / s-1
|1 / a|I
|1 / a|II
|1 / a|III
εI-II
εII-III
10-4
0.49
0.42
0.26
0.084
0.163
10-3
0.43
0.39
0.23
0.079
0.151
10-2
0.41
0.31
0.17
0.066
0.138
10-1
0.37
0.21
0.11
0.061
0.114
Table 3 Strain hardening capacities and transition point strains in each stage for the modified C-J model
1
Tan X D, Ponge D, Lu W J, et al. Carbon and strain partitioning in a quenched and partitioned steel containing ferrite [J]. Acta Mater., 2019, 165: 561
doi: 10.1016/j.actamat.2018.12.019
2
Han Q N, Rui S S, Qiu W H, et al. Crystal orientation effect on fretting fatigue induced geometrically necessary dislocation distribution in Ni-based single-crystal superalloys [J]. Acta Mater., 2019, 179: 129
doi: 10.1016/j.actamat.2019.08.035
3
Li S C, Guo C Y, Hao L L, et al. In-situ EBSD study of deformation behaviour of 600 MPa grade dual phase steel during uniaxial tensile tests [J]. Mater. Sci. Eng., 2019, A759: 624
4
Das A, Tarafder S, Sivaprasad S, et al. Influence of microstructure and strain rate on the strain partitioning behaviour of dual phase steels [J]. Mater. Sci. Eng., 2019, A754: 348
5
Kratochvíl J, Kružík M, Sedláček R. Instability origin of subgrain formation in plastically deformed materials [J]. Int. J. Eng. Sci., 2010, 48: 1401
doi: 10.1016/j.ijengsci.2010.09.017
6
Wang N, Chen Y N, Wu G, et al. Investigation on micromechanism involved in ferrite hardening after prestraining of dual-phase steel [J]. Mater. Sci. Eng., 2021, A800: 140387
7
Dai Q F, Song R B, Fan W Y, et al. Behaviour and mechanism of strain hardening for dual phase steel DP1180 under high strain rate deformation [J]. Acta Metall. Sin., 2012, 48: 1160
doi: 10.3724/SP.J.1037.2012.00364
Shakerifard B, Lopez J G, Legaza M C T, et al. Strain rate dependent dynamic mechanical response of bainitic multiphase steels [J]. Mater. Sci. Eng., 2019, A745: 279
9
Dong D Y, Liu Y, Wang L, et al. Effect of strain rate on dynamic deformation behavior of DP780 steel [J]. Acta Metall. Sin., 2013, 49: 159
doi: 10.3724/SP.J.1037.2012.00515
Kundu A, Field D P, Chakraborti P C. Effect of strain and strain rate on the development of deformation heterogeneity during tensile deformation of a solution annealed 304 LN austenitic stainless steel: An EBSD study [J]. Mater. Sci. Eng., 2020, A773: 138854
11
Ghassemi-Armaki H, Maaß R, Bhat S P, et al. Deformation response of ferrite and martensite in a dual-phase steel [J]. Acta Mater., 2014, 62: 197
doi: 10.1016/j.actamat.2013.10.001
12
Nguyen T T, Park J S, Kim W S, et al. Environment hydrogen embrittlement of pipeline steel X70 under various gas mixture conditions with in situ small punch tests [J]. Mater. Sci. Eng., 2020, A781: 139114
13
Zhang J, Liang Z, Zhao G H. Mechanical behaviour analysis of a buried steel pipeline under ground overload [J]. Eng. Failure Anal., 2016, 63: 131
doi: 10.1016/j.engfailanal.2016.02.008
14
Sodjit S, Uthaisangsuk V. Microstructure based prediction of strain hardening behavior of dual phase steels [J]. Mater. Des., 2012, 41: 370
doi: 10.1016/j.matdes.2012.05.010
15
Chen Y N, Wu Z C, Wu G, et al. Investigation on micromechanism of ferrite hardening after pre-straining with different strain rates of dual-phase steel [J]. Mater. Sci. Eng., 2021, A802: 140657
16
Fillafer A, Krempaszky C, Werner E. On strain partitioning and micro-damage behavior of dual-phase steels [J]. Mater. Sci. Eng., 2014, A614: 180
17
Ma J, Tian C C, Ma A B. Effect on microstructure and properties of X80 high steel grade pipeline steel by prestrain [J]. Ind. Heat., 2021, 50(2): 49
Park S, Jung J, Cho W, et al. Predictive dual-scale finite element simulation for hole expansion failure of ferrite-bainite steel [J]. Int. J. Plast., 2021, 136: 102900
doi: 10.1016/j.ijplas.2020.102900
19
Kuang S, Kang Y L, Yu H, et al. Stress-strain partitioning analysis of constituent phases in dual phase steel based on the modified law of mixture [J]. Int. J. Miner. Metall. Mater., 2009, 16: 393
doi: 10.1016/S1674-4799(09)60070-4
20
Oliver W C, Pharr G M. An improved technique for determining hardness and elastic modulus using load and displacement sensing indentation experiments [J]. J. Mater. Res., 1992, 7: 1564
doi: 10.1557/JMR.1992.1564
21
Zhao Z T, Wang X S, Qiao G Y, et al. Effect of bainite morphology on deformation compatibility of mesostructure in ferrite/bainite dual-phase steel: Mesostructure-based finite element analysis [J]. Mater. Des., 2019, 180: 107870
doi: 10.1016/j.matdes.2019.107870
22
Zhang C Z, Yang S H, Gong B M, et al. Effects of post weld heat treatment (PWHT) on mechanical properties of C-Mn weld metal: Experimental observation and microstructure-based simulation [J]. Mater. Sci. Eng., 2018, A712: 430
23
Werner E, Wesenjak R, Fillafer A, et al. Microstructure-based modelling of multiphase materials and complex structures [J]. Contin. Mech. Thermodyn., 2016, 28: 1325
doi: 10.1007/s00161-015-0477-7
24
Bintu A, Vincze G, Picu C R, et al. Strain hardening rate sensitivity and strain rate sensitivity in TWIP steels [J]. Mater. Sci. Eng., 2015, A629: 54
25
Shamsujjoha M. Evolution of microstructures, dislocation density and arrangement during deformation of low carbon lath martensitic steels [J]. Mater. Sci. Eng., 2020, A776: 139039
26
Feaugas X. On the origin of the tensile flow stress in the stainless steel AISI 316L at 300 K: Back stress and effective stress [J]. Acta Mater., 1999, 47: 3617
doi: 10.1016/S1359-6454(99)00222-0
27
Sedláček R, Blum W. Internal stresses in dislocation subgrain structures [J]. Comput. Mater. Sci., 1998, 13: 148
doi: 10.1016/S0927-0256(98)00055-X
28
Liu X L, Xue Q Q, Wang W, et al. Back-stress-induced strengthening and strain hardening in dual-phase steel [J]. Materialia, 2019, 7: 100376
doi: 10.1016/j.mtla.2019.100376
29
Yang M X, Pan Y, Yuan F P, et al. Back stress strengthening and strain hardening in gradient structure [J]. Mater. Res. Lett., 2016, 4: 145
doi: 10.1080/21663831.2016.1153004
30
Orowan E. Problems of plastic gliding [J]. Proc. Phys. Soc., 1940, 52: 8
doi: 10.1088/0959-5309/52/1/303
31
Zhou N G, Zhou L. Structure and nucleation mechanisms of misfit dislocations in epitaxial FCC thin films with positive and negative mismatches [J]. Mater. Chem. Phys., 2006, 100: 168
doi: 10.1016/j.matchemphys.2005.12.027
32
Olmsted D L, Holm E A, Foiles S M. Survey of computed grain boundary properties in face-centered cubic metals-II: Grain boundary mobility [J]. Acta Mater., 2009, 57: 3704
doi: 10.1016/j.actamat.2009.04.015
33
Liu Q, Fang L M, Xiong Z W, et al. The response of dislocations, low angle grain boundaries and high angle grain boundaries at high strain rates [J]. Mater. Sci. Eng., 2021, A822: 141704
34
Hasan S M, Mandal A, Singh S B, et al. Work hardening behaviour and damage mechanisms in carbide-free bainitic steel during uni-axial tensile deformation [J]. Mater. Sci. Eng., 2019, A751: 142