Effect of Dew Point on Selective Oxidation and Decarburization of 0.2%C-1.5%Si-2.5%Mn High Strength Steel Sheet During Continuous Annealing
JIN Xinyan1,2(), CHU Shuangjie1, PENG Jun1, HU Guangkui1
1.Baoshan Iron and Steel Co., Ltd., Shanghai 201999, China 2.State Key Laboratory of Development and Application Technology of Automotive Steels, Baosteel, Shanghai 201999, China
Cite this article:
JIN Xinyan, CHU Shuangjie, PENG Jun, HU Guangkui. Effect of Dew Point on Selective Oxidation and Decarburization of 0.2%C-1.5%Si-2.5%Mn High Strength Steel Sheet During Continuous Annealing. Acta Metall Sin, 2023, 59(10): 1324-1334.
The use of advanced high strength steel (AHSS) sheets has been acknowledged as an important solution for vehicle weight reduction, and thus, carbon dioxide emission reduction. The development of third-generation AHSS has become one of the steel industry's most prominent concerns in recent years. However, the selective oxidation of alloy components such as silicon and manganese makes obtaining high-quality hot-dipped galvanized steel sheets extremely difficult. To determine an optimal process window for controlling the surface microstructure of AHSS, the effect of dew point on selective oxidation of silicon and manganese, and decarburization in a 0.2%C-1.5%Si-2.5%Mn (mass fraction) steel sheet was studied by performing continuous annealing simulation experiments. Glow discharge optical emission spectrometry (GD-OES) was used to determine the depth profiles of alloy elements, and SEM and OM were used to determine the depths of internal oxidation and decarburization zones in the subsurface. The surface and internal oxides' precise microstructures were studied using TEM on a FIB-prepared cross-sectional specimen. The increasing dew point of the atmosphere through the heating and soaking section portion of continuous annealing results in the transformation of external oxidation of silicon and manganese to internal oxidation. When the steel was annealed in an environment with a dew point of -40oC, a continuous silicon, manganese external oxidation layer with an average thickness of 40-50 nm covered the surface. When the dew point was elevated to +10oC, a subsurface oxidation layer approximately 5-μm thick formed. Due to the substantially lower oxygen pressure required for the Si/SiO2 equilibrium, the internal oxides exhibited a core-shell structure consisting of a Si-rich oxide core and a surrounding Mn-Si mixed oxide shell. A higher dew point results in the formation of an obvious decarburization layer in the subsurface, which is visible as a layer of ferrite grains with significantly decreased microhardness. When the dew point was increased from -40oC to +10oC, the thickness of the decarburized zone increased from 0 μm to 45 μm, and the C content of the decarburized zone decreased from 0.18% to 0.01%. External oxidation can no longer be decreased further by increasing the dew point, yet the depth of internal oxidation and decarburization in the subsurface continues to increase. Therefore, maintaining an appropriate dew point range for the annealing atmosphere is necessary to manage external oxidation and decarburization. The optimal dew point should be adjusted between -20oC and -10oC when annealed at 870oC for 120 s in 5%H2-N2 atmosphere.
Fig.1 Thermal cycle of the annealing experiments (Td—dew point)
Fig.2 Fe, Mn, Si, and O depth profiles of the sample annealed at dew point of -40oC (pMn—peak value of Mn, pSi—peak value of Si, te—thickness of external oxidation)
Fig.3 Mn (a) and Si (b) depth profiles of the samples annealed at different dew points
Fig.4 Effects of dew point on the external and internal oxidations of Mn and Si (ti—thickness of internal oxidation) (a) pMn and pSi (b) te and ti
Fig.5 Cross-sectional SEM images of the samples annealed at different dew points (a) -40oC (b) -20oC (c) 0oC (d) +10oC
Fig.6 TEM image of the focused ion beam (FIB) prepared cross-sectional sample annealed at dew point of -40oC (a) and enlarged images of zone 1 (b), zone 2 (c), and zone 3 (d)
Fig.7 EDS elemental mapping of the TEM sample annealed at dew point of -40oC
Fig.8 TEM image of the FIB prepared cross-sectional sample annealed at dew point of +10oC (a) and enlarged images of zone 1 (b), zone 2 (c), and zone 3 (d)
Fig.9 EDS elemental mapping of three different areas (in Fig.8a) on the sample annealed at dew point of +10oC (a) upper zone (b) middle zone (c) bottom zone
Fig.10 C depth profiles of the samples annealed at different dew points
Fig.11 Effects of dew point on C content (a) and decar-burization thickness (b) in the subsurface area (td1—thickness of total decarburization, td2—thickness of full decarburization)
Fig.12 Cross-sectional OM images of the samples annealed at different dew points (a) -40oC (b) -20oC (c) 0oC (d) +10oC
Fig.13 Effects of dew point on microhardness along the depth in the subsurface area
Fig.14 Schematic diagram showing the effect of dew point on selective oxidation and decarburization of 0.2C-1.5Si-2.5Mn high strength steel sheet during continuous annealing at the dew points of -40oC (a) and +10oC (b)
Td / oC
T / oC
/ atm
/ atm
/ atm
-40
870
0.05
1.27 × 10-4
8.08 × 10-23
-20
870
0.05
1.02 × 10-3
5.20 × 10-21
0
870
0.05
6.03 × 10-3
1.82 × 10-19
+10
870
0.05
1.21 × 10-2
7.37 × 10-19
Table 1 Calculated partial oxygen pressures as a function of dew point
Element
Temperature
Diffusion coefficient
oC
μm2·s-1
O
870
1.507 × 101
Mn
870
4.227 × 10-3
Si
870
6.615 × 10-3
C
870
2.551 × 101
Table 2 Diffusion coefficients of O, Mn, Si, and C in steel
Fig.15 Effect of dew point on te,ti, td1, and wC (wC—C content of surface area)
1
Bouaziz O, Zurob H, Huang M X. Driving force and logic of development of advanced high strength steels for automotive applications [J]. Steel Res. Int., 2013, 84: 937
doi: 10.1002/srin.v84.10
2
Meknassi R F, Miklós T. Third generation of advanced high strength sheet steels for the automotive sector: A literature review [J]. Multidiszciplin. Tudom., 2021, 11: 241
3
Pednekar V, Khutorsky A, Lad S, et al. Third generation 980 class AHSS: A viable alternative to replace press-hardenable steels (PHS) in automotive rear rail applications [R]. SAE Tech. Pap., doi: 10.4271/2020-01-0534
4
Wang C Y, Yang J, Chang Y, et al. Development trend and challenge of advanced high strength automobile steels [J]. Iron Steel, 2019, 54(2): 1
Chen Z, He Y L, Zheng W S, et al. Effect of hot-dip galvanizing process on selective oxidation and galvanizability of medium manganese steel for automotive application [J]. Coatings, 2020, 10: 1265
doi: 10.3390/coatings10121265
7
Jin X Y, Hu G K, Qian H W, et al. Effect of dew point on galvanizability in 4 mass% Al added low density steel [J]. ISIJ Int., 2018, 58: 1584
doi: 10.2355/isijinternational.ISIJINT-2018-010
8
Samanta S, Halder A K, Deo Y, et al. Effect of Mn and Cr on the selective oxidation, surface segregation and hot-dip Zn coatability [J]. Surf. Coat. Technol., 2019, 377: 124908
doi: 10.1016/j.surfcoat.2019.124908
9
Zhou D Y, Li M, Mi Z L, et al. Investigation of selective oxidation and reaction wetting of Q&P steel under different dew point during continuous galvanizing [J]. Trans. Indian Inst. Met., 2021, 74: 235
doi: 10.1007/s12666-020-02141-1
10
Song G M, Sloof W G, Vystavel T, et al. Interface microstructure and adhesion of zinc coatings on TRIP steels [J]. Mater. Sci. Forum, 2007, 539-543: 1104
doi: 10.4028/www.scientific.net/MSF.539-543
11
Jin X Y, Chen J J, Hu G K, et al. Investigation on the coating adhesion of galvanized AHSS treated by oxidation-reduction process [J]. Iron Steel Technol., 2020, 17: 108
12
Hao Y L, Cai N, Yao S C, et al. Effect of selective oxidation behavior of high strength dual-phase steel surface on phosphating properties [J]. Surf. Technol., 2020, 49(8): 309
Liu H C, He Y L, Li L. Application of thermodynamics and Wagner model on two problems in continuous hot-dip galvanizing [J]. Appl. Surf. Sci., 2009, 256: 1399
doi: 10.1016/j.apsusc.2009.08.095
14
Zhang X, Da Silva C C, Liu C, et al. Selective oxidation of ternary Fe-Mn-Si alloys during annealing process [J]. Corros. Sci., 2020, 174: 108859
doi: 10.1016/j.corsci.2020.108859
15
Fushiwaki Y, Kawano T, Nagataki Y. Influence of Cr addition on selective oxidation behavior of Mn-added high-strength steel sheet [J]. ISIJ Int., 2018, 58: 1623
doi: 10.2355/isijinternational.ISIJINT-2018-075
16
Story M E, Webler B A. Effects of surface microstructure on selective oxidation morphology and kinetics in N2 + 5% H2 atmosphere with variable dew point temperature [J]. ISIJ Int., 2019, 59: 918
doi: 10.2355/isijinternational.ISIJINT-2018-727
17
Mousavi G S, McDermid J R. Selective oxidation of a C-2Mn-1.3Si (wt pct) advanced high-strength steel during continuous galvanizing heat treatments [J]. Metall. Mater. Trans., 2018, 49A: 5546
18
Pourmajidian M, McDermid J R. Selective oxidation of a 0.1C-6Mn-2Si third generation advanced high-strength steel during dew-point controlled annealing [J]. Metall. Mater. Trans., 2018, 49A: 1795
19
Lu R, Wu G X, Zhang J Y. Phase equilibrium calculation of water pressure control in hydrogen reduction system [J]. J. Iron Steel Res. Int., 2021, 33: 119
Jiang G R, Wang H Q, Liu L B, et al. Effects of heating atmosphere on selective oxidation of a C-Mn-Si-Al high strength steel [J]. Iron and Steel, 2018, 53(3): 66
Wu G X, Zhang J Y. Effect of water pressure and soaking time on the selective oxidation of DP980 advanced high strength steel [J]. Appl. Surf. Sci., 2018, 453: 252
doi: 10.1016/j.apsusc.2018.05.034
22
Zhang Z T, Sohn I R, Pettit F S, et al. Investigation of the effect of alloying elements and water vapor contents on the oxidation and decarburization of transformation-induced plasticity steels [J]. Metall. Mater. Trans., 2009, 40B: 567
23
Han X, DiGiovanni C, McDermid J, et al. Effect of internal oxidation on the weldability of CMnSi steels [J]. Weld. World, 2019, 63: 1633
doi: 10.1007/s40194-019-00798-x
24
Kalashami A G, DiGiovanni C, Razmpoosh M H, et al. The role of internal oxides on the liquid metal embrittlement cracking during resistance spot welding of the dual phase steel [J]. Metall. Mater. Trans., 2020, 51A: 2180
25
Kalashami A G, Han X, Goodwin F, et al. The influence of modified annealing during the galvanizing process on the resistance spot welding of the CMn1.8Si advanced high strength steel [J]. Surf. Coat. Technol., 2020, 381: 125181
doi: 10.1016/j.surfcoat.2019.125181
26
Li Y P. A study on selective oxidation behaviors of DP780 dual phase steels during hot-dip galvanizing process [D]. Beijing: China iron and Steel Research Institute Group, 2012
李远鹏. 热镀锌DP780双相钢的选择性氧化行为研究 [D]. 北京: 钢铁研究总院, 2012
27
Huin D, Flauder P, Leblond J B. Numerical simulation of internal oxidation of steels during annealing treatments [J]. Oxid. Met., 2005, 64: 131
doi: 10.1007/s11085-005-5718-x
28
Lee S J, Matlock D K, Van Tyne C J. An empirical model for carbon diffusion in austenite incorporating alloying element effects [J]. ISIJ Int., 2011, 51: 1903
doi: 10.2355/isijinternational.51.1903
29
Zhang K, Chen Y L, Sun Y H, et al. Effect of H2O(g) on decarburization of 55SiCr spring steel during the heating process [J]. Acta Metall. Sin., 2018, 54: 1350
Hasegawa M. Ellingham Diagram [A]. Treatise on Process Metallurgy Vol. 1 [M]. Boston: Elsevier, 2014: 507
31
Gong Y F, Kim H S, De Cooman B C. Formation of surface and subsurface oxides during ferritic, intercritical and austenitic annealing of CMnSi TRIP steel [J]. ISIJ Int., 2008, 48: 1745
doi: 10.2355/isijinternational.48.1745