Acta Metall Sin  2019, Vol. 55 Issue (3): 308-316    DOI: 10.11900/0412.1961.2018.00136
Current Issue | Archive | Adv Search |
Effect of Nitrogen Doping on Microstructure and Wear Resistance of Tantalum Coatings Deposited by Direct Current Magnetron Sputtering
Shasha YANG1,2,Feng YANG3,Minghui CHEN4(),Yunsong NIU1,Shenglong ZHU1,Fuhui WANG4
1. Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
2. School of Material Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
3. School of Equipment Engineering, Shenyang Ligong University, Shenyang 110159, China
4. Shenyang National Key Laboratory for Materials Science, Northeastern University, Shenyang 110819, China
Cite this article: 

Shasha YANG,Feng YANG,Minghui CHEN,Yunsong NIU,Shenglong ZHU,Fuhui WANG. Effect of Nitrogen Doping on Microstructure and Wear Resistance of Tantalum Coatings Deposited by Direct Current Magnetron Sputtering. Acta Metall Sin, 2019, 55(3): 308-316.

Download:  HTML  PDF(17619KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

Tantalum coating attracts increasing attention in heat, corrosion and wear resistant applications today because of its high melting point, immunity to chemical attack and high toughness. Recently, tantalum has been considered a desirable candidate to replace electrodeposited (ED) chromium coating which is often used as protective coating against corrosion and wear. However, the wastes associated with ED chromium contain a well-known carcinogen, i.e. hexavalent chromium, which is a hazard to environment. In comparison, thick Ta coating is regarded as a more environmental and beneficial replacement. Tantalum coating is usually obtained by magnetron sputtering. However, tantalum exhibits two distinct crystalline phases. The body-centered cubic α-phase is the common phase in bulk metal and thermodynamically stable. α-Ta with good ductility and excellent mechanical properties is welcomed in most fields. β-Ta is a metastable phase with tetragonal crystalline lattice structure. The properties of β-Ta are not as advantageous as α-Ta because it is hard and brittle. The existence of β-Ta may compromise tantalum coating in adhesion, corrosion and wear resistance, hence, finding appropriate deposition conditions to obtain pure α-phase Ta coating has attracted a lot of interests. In previous work, pure α-phase Ta coating has been deposited by direct current magnetron sputtering when substrates were located in negative glow space. In this work, nitrogen was mixed in sputtering gases to deposit Ta coating with N interstitially dissolved on stainless steel. Effect of N on microstructure, mechanical and tribological performance of Ta coating was studied. Results indicated that when no nitrogen or very low flux of N2 (l mL/s) were introduced in gas mixtures, α-phase Ta coating with coarse grains grew and revealed strong reflections of (211) and (110) diffraction peaks. When N2 flow rate reached to 5 mL/s, Ta coating with N interstitially dissolved was obtained and revealed grain refinement and (110) preferred orientation of TaN0.1 phase. Compared to α-phase Ta coating, N-doped tantalum coatings displayed excellent wear resistance for their high hardness and H 3/E 2 ratio (H—hardness, E—elastic modulus). The wear mechanism for α-Ta coating was abrasive wear, while that of N-doped Ta coating switched to adhesive wear.

Key words:  Ta coating      magnetron sputtering      nitrogen doping      wear     
Received:  11 April 2018     
ZTFLH:  TG174.4  
Fund: National Key Research and Development Program of China(2017YFB0306100);National Key Research and Development Program of China (No.2017YFB0306100), National Natural Science Foundation of China(51671053);National Key Research and Development Program of China (No.2017YFB0306100), National Natural Science Foundation of China(51701223);Joint Fund of the Equipment Pre-Research and the Ministry of Education(6141A020332-004);Fundamental Research Funds for the Central Universities(N160205001)

URL: 

https://www.ams.org.cn/EN/10.11900/0412.1961.2018.00136     OR     https://www.ams.org.cn/EN/Y2019/V55/I3/308

Coating

Ar flow rate

mL·s-1

N2 flow rate

mL·s-1

Cathode power

kW

Deposition temperature

℃

Base pressure

Pa

Sputtering

pressure

Pa

Deposition time

h

10Ar1002.02005.0×10-32.3×10-14
10Ar-1N21012.02005.0×10-32.3×10-14
10Ar-5N21052.02005.0×10-32.4×10-14
15Ar1502.02005.0×10-33.4×10-14
15Ar-5N21552.02005.0×10-33.5×10-14
Table 1  Deposition parameters of Ta and N-doped Ta coatings
Fig.1  Surface (a, c, e, g, i) and cross-sectional (b, d, f, h, j) SEM images of as-deposited Ta coatings with different Ar and N2 fluxes (Insets in Figs.1a, c, e, g and i show the enlarged views)(a, b) 10Ar (c, d) 10Ar-1N2 (e, f) 10Ar-5N2 (g, h) 15Ar (i, j) 15Ar-5N2
Fig.2  TEM images of as-deposited 15Ar (a) and 15Ar-5N2 (b) coatings in planar view (Insets show the corresponding SAED patterns of the circle regions)
Fig.3  XRD spectra of as-deposited Ta coatings with different Ar and N2 fluxes
Fig.4  XPS result of the Ta4f photoelectron peak for the as-deposited 15Ar-5N2 coating

Coating

Hardness

GPa

Elastic modulus

GPa

H/E

H3/E2

Wear Rate

10-2 mg·N-1·m-1

10Ar8.159212.4210.03840.01201.333
10Ar-1N212.396237.5700.05220.03370.167
10Ar-5N219.851266.4520.07450.11020.133
15Ar7.885233.8450.03370.00901.483
15Ar-5N221.569294.2570.07330.1159-0.017
Table 2  Mechanical properties and wear rates of as-deposited Ta coatings
Fig.5  Worn surface SEM images of Ta coatings deposited under different Ar and N2 fluxes(a) 10Ar (b) 10Ar-1N2 (c) 10Ar-5N2 (d) 15Ar (e) 15Ar-5N2
Fig.6  Enlarged worn scar of the rectangular region in Fig.5b (a) and the corresponding EDS analyses of elements O (b), Fe (c) and Ta (d)
Fig.7  Schematics of wear mechanisms for Ta coatings (FN—vertical load, V—sliding velocity)(a) none N-doped Ta coating (b) N-doped Ta coating
[1] Sopok S, Rickard C, Dunn S. Thermal-chemical-mechanical gun bore erosion of an advanced artillery system part one: Theories and mechanisms [J]. Wear, 2005, 258: 659
[2] Chen X J, Yan Q, Ma Q, Influence of the laser pre-quenched substrate on an electroplated chromium coating/steel substrate [J]. Appl. Surf. Sci., 2017, 405: 273
[3] Van Phuong N, Kwon S C, Lee J Y, et al. The effects of pH and polyethylene glycol on the Cr(III) solution chemistry and electrodeposition of chromium [J]. Surf. Coat. Technol., 2012, 206: 4349
[4] Quan C, He Y D. Properties of nanocrystalline Cr coatings prepared by cathode plasma electrolytic deposition from trivalent chromium electrolyte [J]. Surf. Coat. Technol., 2015, 269: 319
[5] Lee S L, Windover D, Audino M, et al. High-rate sputter deposited tantalum coating on steel for wear and erosion mitigation [J]. Surf. Coat. Technol., 2002, 149: 62
[6] Maeng S M, Axe L, Tyson T A, et al. Corrosion behavior of magnetron sputtered α-Ta coatings on smooth and rough steel substrates [J]. Surf. Coat. Technol., 2006, 200: 5717
[7] Hu X F, Xu Q. Preparation of tantalum by electro-deoxidation in a CaCl2-NaCl melt [J]. Acta Metall. Sin., 2006, 42: 285
[7] 胡小锋, 许 茜. CaCl2-NaCl熔盐电脱氧法制备金属Ta [J]. 金属学报, 2006, 42: 285
[8] Matson D W, McClanahan E D, Lee S L, et al. Properties of thick sputtered Ta used for protective gun tube coatings [J]. Surf. Coat. Technol., 2001, 146-147: 344
[9] Wang S, Xiong D S, Li J L, et al. Wear and erosion resistance properties of electroplating Ta coating in molten salt [J]. China Surf. Eng., 2015, 28(2): 101
[9] 王 升, 熊党生, 李建亮等. 熔盐电镀钽及其耐磨损烧蚀性能 [J]. 中国表面工程, 2015, 28(2): 101
[10] Myers S, Lin J L, Souza R M, et al. The β to α phase transition of tantalum coatings deposited by modulated pulsed power magnetron sputtering [J]. Surf. Coat. Technol., 2013, 214: 38
[11] Lundin D, Sarakinos K. An introduction to thin film processing using high-power impulse magnetron sputtering [J]. J. Mater. Res., 2012, 27: 780
[12] Lin J L, Moore J J, Sproul W D, et al. Effect of negative substrate bias on the structure and properties of Ta coatings deposited using modulated pulse power magnetron sputtering [J]. IEEE Trans. Plasma Sci., 2010, 38: 3071
[13] Ferreira F, Sousa C, Cavaleiro A, et al. Phase tailoring of tantalum thin films deposited in deep oscillation magnetron sputtering mode [J]. Surf. Coat. Technol., 2017, 314: 97
[14] Frank S, Gruber P A, Handge U A, et al. In situ studies on the cohesive properties of α- and β-Ta layers on polyimide substrates [J]. Acta Mater., 2011, 59: 5881
[15] Niu Y S, Chen M H, Wang J L, et al. Preparation and thermal shock performance of thick α-Ta coatings by direct current magnetron sputtering (DCMS) [J]. Surf. Coat. Technol., 2017, 321: 19
[16] Lou B Y, Wang Y X. Effects of Mo content on the micro-structure and tribological properties of CrMoAlN films [J]. Acta Metall. Sin., 2016, 52: 727
[16] 楼白杨, 王宇星. Mo含量对CrMoAlN薄膜微观结构和摩擦磨损性能的影响 [J]. 金属学报, 2016, 52: 727
[17] Han K C, Liu Y Q, Lin G Q, et al. Study on atomic-scale strengthening mechanism of transition-metal nitride MNx(M=Ti,Zr,Hf) films within wide composition ranges [J]. Acta Metall. Sin., 2016, 52: 1601
[17] 韩克昌, 刘一奇, 林国强等. 宽固溶区过渡金属氮化物MNx(M=Ti, Zr, Hf)硬质薄膜原子尺度强化机制研究 [J]. 金属学报, 2016, 52: 1601
[18] Cui W F, Cao D, Qin G W. Microstructure and wear resistance of Ti/TiN multilayer films deposited by magnetron sputtering [J]. Acta Metall. Sin., 2015, 51: 1531
[18] 崔文芳, 曹 栋, 秦高悟. 磁控溅射沉积Ti/TiN多层膜的组织特征及耐磨损性能 [J]. 金属学报, 2015, 51: 1531
[19] Zhao S L, Zhang Z, Zhang J, et al. Microstructure and wear resistance of TiAlZrCr/(Ti, Al, Zr, Cr)N gradient films deposited by multi-arc ion plating [J]. Acta Metall. Sin., 2016, 52: 747
[19] 赵时璐, 张 震, 张 钧等. 多弧离子镀TiAlZrCr/(Ti, Al, Zr, Cr)N梯度膜的微观结构与耐磨损性能 [J]. 金属学报, 2016, 52: 747
[20] Raole P M, Narsale A M, Kothari D C, et al. Glancing-angle X-ray diffraction and X-ray photoelectron spectroscopy studies of nitrogen-implanted tantalum [J]. Mater. Sci. Eng., 1989, A115: 73
[21] Rogers J D, Sundaram V S, Kleiman G G, et al. High resolution study of the M45N67N67 and M45N45N67 Auger transitions in the 5d series [J]. J. Phys., 1982, 12F: 2097
[22] Takano I, Isobe S, Sasaki T A, et al. Nitrogenation of various transition metals by N+2-ion implantation [J]. Appl. Surf. Sci., 1989, 37: 25
[23] Stavrev M, Fischer D, Wenzel C, et al. Crystallographic and morphological characterization of reactively sputtered Ta, Ta-N and Ta-N-O thin films [J]. Thin Solid Films, 1997, 307: 79
[24] Zhu S L, Wang F H, Wu W T. Theory and Application of Reactive Sputtering Kinetics [M]. Beijing: China Science and Technology Press, 1999: 18
[24] 朱圣龙, 王福会, 吴维?. 反应溅射动力学理论及应用 [M]. 北京: 中国科学技术出版社, 1999: 18
[25] Pelleg J, Zevin L Z, Lungo S, et al. Reactive-sputter-deposited TiN films on glass substrates [J]. Thin Solid Films, 1991, 197: 117
[26] Wang X, Wang Z Y, Feng Z X, et al. Effect of N doping on microstructure, mechanical and tribological properties of V-Al-C coatings [J]. Acta Metall. Sin., 2017, 53: 709
[26] 王 鑫, 王振玉, 冯再新等. N掺杂对V-Al-C涂层微观结构、力学及摩擦性能的影响 [J]. 金属学报, 2017, 53: 709
[27] Xu S, Xu J, Munroe P, et al. Nanoporosity improves the damage tolerance of nanostructured tantalum nitride coatings [J]. Scr. Mater., 2017, 133: 86
[28] Hakamada M, Nakamoto Y, Matsumoto H, et al. Relationship between hardness and grain size in electrodeposited copper films [J]. Mater. Sci. Eng., 2007, A457: 120
[29] Yamamoto T, Kawate M, Hasegawa H, et al. Effects of nitrogen concentration on microstructures of WNx films synthesized by cathodic arc method [J]. Surf. Coat. Technol., 2005, 193: 372
[30] Cheng G A, Han D Y, Liang C L, et al. Influence of residual stress on mechanical properties of TiAlN thin films [J]. Surf. Coat. Technol., 2013, 228: S328
[31] Yu L H, Dong H Z, Xu J H. Influence of C content on microstructure, mechanical properties and friction and wear properties of TiWCN composite films [J]. Acta Metall. Sin., 2014, 50: 1350
[31] 喻利花, 董鸿志, 许俊华. C含量对TiWCN复合膜微结构、力学性能和摩擦磨损性能的影响 [J]. 金属学报, 2014, 50: 1350
[32] Aliofkhazraei M, Rouhaghdam A S. Fabrication of TiC/WC ultra hard nanocomposite layers by plasma electrolysis and study of its characteristics [J]. Surf. Coat. Technol., 2010, 205: S51
[1] HUANG Ding, QIAO Yanxin, YANG Lanlan, WANG Jinlong, CHEN Minghui, ZHU Shenglong, WANG Fuhui. Effect of Shot Peening of Substrate Surface on Cyclic Oxidation Behavior of Sputtered Nanocrystalline Coating[J]. 金属学报, 2023, 59(5): 668-678.
[2] FENG Li, WANG Guiping, MA Kai, YANG Weijie, AN Guosheng, LI Wensheng. Microstructure and Properties of AlCo x CrFeNiCu High-Entropy Alloy Coating Synthesized by Cold Spraying Assisted Induction Remelting[J]. 金属学报, 2023, 59(5): 703-712.
[3] MIAO Junwei, WANG Mingliang, ZHANG Aijun, LU Yiping, WANG Tongmin, LI Tingju. Tribological Properties and Wear Mechanism of AlCr1.3TiNi2 Eutectic High-Entropy Alloy at Elevated Temperature[J]. 金属学报, 2023, 59(2): 267-276.
[4] WANG Haifeng, ZHANG Zhiming, NIU Yunsong, YANG Yange, DONG Zhihong, ZHU Shenglong, YU Liangmin, WANG Fuhui. Effect of Pre-Oxidation on Microstructure and Wear Resistance of Titanium Alloy by Low Temperature Plasma Oxynitriding[J]. 金属学报, 2023, 59(10): 1355-1364.
[5] ZHANG Shihong, HU Kai, LIU Xia, YANG Yang. Corrosion-Erosion Mechanism and Research Prospect of Bare Materials and Protective Coatings for Power Generation Boiler[J]. 金属学报, 2022, 58(3): 272-294.
[6] HAN Ruyang, YANG Gengwei, SUN Xinjun, ZHAO Gang, LIANG Xiaokai, ZHU Xiaoxiang. Austenite Grain Growth Behavior of Vanadium Microalloying Medium Manganese Martensitic Wear-Resistant Steel[J]. 金属学报, 2022, 58(12): 1589-1599.
[7] CUI Hongzhi, JIANG Di. Research Progress of High-Entropy Alloy Coatings[J]. 金属学报, 2022, 58(1): 17-27.
[8] CAO Qingping, LV Linbo, WANG Xiaodong, JIANG Jianzhong. Magnetron Sputtering Metal Glass Film Preparation and the “Specimen Size Effect” of the Mechanical Property[J]. 金属学报, 2021, 57(4): 473-490.
[9] BI Jiazi, LIU Xiaobin, LI Ran, ZHANG Tao. Tribological Properties of Polyalphaolefin (PAO6) Lubricant Modified with Particles Additives of Metallic Glass[J]. 金属学报, 2021, 57(4): 559-566.
[10] LI Xiaoqian, WANG Fuguo, LIANG Aimin. Effect of Spraying Process on Microstructure and Tribological Properties of Ta2O5 In Situ Composite Nanocrystalline Ta-Based Coatings[J]. 金属学报, 2021, 57(2): 237-246.
[11] ZHAO Wanxin, ZHOU Zheng, HUANG Jie, YANG Yange, DU Kaiping, HE Dingyong. Microstructure and Frictional Wear Behavior of FeCrNiMo Alloy Layer Fabricated by Laser Cladding[J]. 金属学报, 2021, 57(10): 1291-1298.
[12] SUN Xinjun,LIU Luojin,LIANG Xiaokai,XU Shuai,YONG Qilong. TiC Precipitation Behavior and Its Effect on Abrasion Resistance of High Titanium Wear-Resistant Steel[J]. 金属学报, 2020, 56(4): 661-672.
[13] WEI Shizhong, XU Liujie. Review on Research Progress of Steel and Iron Wear-Resistant Materials[J]. 金属学报, 2020, 56(4): 523-538.
[14] WU Xiang,ZUO Xiurong,ZHAO Weiwei,WANG Zhongyang. Mechanism of TiN Fracture During the Tensile Process of NM500 Wear-Resistant Steel[J]. 金属学报, 2020, 56(2): 129-136.
[15] XU Shuai, SUN Xinjun, LIANG Xiaokai, LIU Jun, YONG Qilong. Effect of Hot Rolling Deformation on Microstructure and Mechanical Properties of a High-Ti Wear-Resistant Steel[J]. 金属学报, 2020, 56(12): 1581-1591.
No Suggested Reading articles found!