INFLUENCE OF THE COMPOSITION OF Zn-Al FILLER METAL ON THE INTERFACIAL STRUCTURE AND PROPERTY OF Cu/Zn-Al/Al BRAZED JOINT
YANG Hao1, HUANG Jihua1(), CHEN Shuhai1, ZHAO Xingke1, WANG Qi2, LI Dehua2
1 School of Materials Science and Engineering, University of Science and Technology Beijing, Beijing 100083 2 Gree Electric Appliances, Inc. of Zhuhai, Zhuhai 519070
Cite this article:
YANG Hao, HUANG Jihua, CHEN Shuhai, ZHAO Xingke, WANG Qi, LI Dehua. INFLUENCE OF THE COMPOSITION OF Zn-Al FILLER METAL ON THE INTERFACIAL STRUCTURE AND PROPERTY OF Cu/Zn-Al/Al BRAZED JOINT. Acta Metall Sin, 2015, 51(3): 364-370.
The Cu/Al dissimilar metal joint is a compound structure that can efficiently decrease manufacturing costs, reduce product weight, and integrate the advantages of both metals. For the excellent comprehensive properties, the Cu/Al dissimilar metal joint has broad application prospects in air conditioners, refrigerators, cables, electronic components, solar collectors, et al. Brazing is considered as a promising method to join the Cu/Al dissimilar metal for lower residual stress, lower costs, higher precision and better adaption to the structure of joint. Meanwhile, the Zn-Al filler metal is considered as the relatively ideal filler metal due to better property of the Cu/Zn-Al/Al joint. However, the influence of the composition of the Zn-Al filler metal on the interfacial structure near Cu substrate and property of the Cu/Al joint has not been investigated. In this work, the Cu/Al joints were brazed by Zn-15Al, Zn-22Al, Zn-28Al, Zn-37Al and Zn-45Al filler metals, respectively. The influences of the composition of Zn-Al filler metals on the interfacial structure near Cu substrate of the Cu/Al joints were investigated, and the relationships of the composition of the Zn-Al filler metals, the interfacial structure and the shear strength of the Cu/Al joints were described systematically. It was found that the interfacial structure of the Cu/Zn-15Al/Al brazed joint was Cu/Al4.2Cu3.2Zn0.7. For thinner Al4.2Cu3.2Zn0.7 layer (2~3 μm), the shear strength of the joint was higher (66.3 MPa). With the increase of Al content of the filler metal, the thickness of Al4.2Cu3.2Zn0.7 layer at the interface was increased for Cu/Zn-22Al/Al joint, even some CuAl2 phase can be found nearby the Al4.2Cu3.2Zn0.7 layer of Cu/Zn-28Al/Al joint, and the shear strength of the Cu/Al joints were decreased correspondingly. When the Cu/Al joint was brazed by the Zn-37Al filler metal, the interfacial structure near Cu substrate was transformed into Cu/Al4.2Cu3.2Zn0.7/CuAl2. For higher brittleness of CuAl2 layer, the shear strength of the joint was decreased obviously (34.5 MPa). Finally, the interfacial structure of the Cu/Zn-45Al/Al joint was transformed into Cu/CuAl2, the interfacial structure lead to the lower shear strength of the joint, which is only 31.6 MPa.
Table 1 Melting points and brazing temperatures of the Zn-Al filler metals
Fig.1 Schematic of the brazed specimen
Fig.2 SEM images of the interfacial zones near Cu substrate of the Cu/Al joints brazed with Zn-15Al (a), Zn-22Al (b), Zn-28Al (c), Zn-37Al (d) and Zn-45Al (e)
Filler metal
Position
Atomic fraction / %
Possible phase
Al
Cu
Zn
Zn-15Al
A
55.15
34.12
10.23
Al4.2Cu3.2Zn0.7
Zn-22Al
B
55.00
35.96
9.03
Al4.2Cu3.2Zn0.7
C
68.34
28.26
3.40
CuAl2
Zn-28Al
D
53.77
35.34
10.89
Al4.2Cu3.2Zn0.7
E
67.88
26.77
5.35
CuAl2
Zn-37Al
F
55.14
37.59
7.27
Al4.2Cu3.2Zn0.7
G
67.99
29.25
2.77
CuAl2
Zn-45Al
H
56.33
38.50
5.17
Al4.2Cu3.2Zn0.7
I
69.09
28.94
1.96
CuAl2
Fig.3 XRD spectra of the interfacial zones near Cu substrate of the Cu/Al joints brazed with Zn-15Al (a), Zn-22Al (b) and Zn-37Al (c)
Fig.4 Shear strength of Cu/Al joints brazed with Zn-Al filler metals
Fig.5 Fractographs of the Cu/Al joints brazed with Zn-15Al (a), Zn-22Al (b), Zn-28Al (c), Zn-37Al (d) and Zn-45Al (e)
[1]
Liu P, Shi Q Y, Wang W, Wang X, Zhang Z L. Mater Lett, 2008; 62: 4106
[2]
Xue P, Ni D R, Wang D, Xiao B L, Ma Z Y. Mater Sci Eng, 2011; A528: 4683
[3]
Zuo D, Hu S S, Shen J Q, Xue Z Q. Mater Des, 2014; 58: 357
[4]
Mai T A, Spowage A C. Mater Sci Eng, 2004; A374: 224
[5]
Xue P, Xiao B L, Ni D R, Ma Z R. Mater Sci Eng, 2010; A527: 5723
[6]
Matsuoka S, Imai H. J Mater Process Technol, 2009; 209: 954
[7]
Eslami P, Taheri K A. Mater Lett, 2011; 65: 1862
[8]
Lee T H, Lee Y J, Park K T, Nersisyan H H, Jeong H G, Lee J H. J Mater Process Technol, 2013; 213: 487
[9]
Xia C Z, Li Y J, Puchkov U A, Gerasimov S A, Wang J. Vacuum, 2008; 82: 799
[10]
Huang M L, Kang N, Zhou Q, Huang Y Z. J Mater Sci Technol, 2012; 28: 844
[11]
Berlanga L C, Albístur G A, Balerdi A P, Gutiérrez P M, Fernández C J. Manuf Process, 2011; 26: 236
[12]
Xiao Y, Ji H J, Li M Y, Kim J Y. Mater Des, 2013; 52: 740
[13]
Ji F, Xue S B, Dai W. Mater Des, 2012; 42: 156
[14]
Ji F, Xue S B, Dai W. Rare Met Mater Eng, 2013; 42: 2453
[15]
Zhang Q Y,Zhuang H S. Brazing and Soldering Manual. Beijing: China Machine Press, 2008: 498
(张启运,庄鸿寿. 钎焊手册. 北京: 机械工业出版社, 2008: 498)
[16]
Yan X Q, Liu S X, Long W M, Huang J L, Zhang L Y, Chen Y. Mater Lett, 2013; 93: 183
[17]
Zhang M, Xue S B, Ji F, Lou Y B, Wang S Q. Trans China Weld Inst, 2011; 32(2): 93
(张 满, 薛松柏, 姬 峰, 娄银斌, 王水庆. 焊接学报, 2011; 32(2): 93)
[18]
Zhang M, Xue S B, Ji F, Lou Y B, Wang S Q. Trans China Weld Inst, 2010; 31(9): 73
(张 满, 薛松柏, 姬 峰, 楼银斌, 王水庆. 焊接学报, 2010; 31(9): 73)
[19]
Liu R. Master Thesis, Jiangsu University of Science and Technology, ZhenJiang, 2012
(刘 日. 江苏科技大学硕士学位论文, 镇江, 2012)
[20]
Yan X Q, Liu S X, Long W M, Huang J L, Zhang L Y, Chen Y. Mater Lett, 2013; 93: 183
[21]
Chen Z,Zhou F,Wang G F. Principle of Joining and Welding. Harbin: Harbin Institute of Technology Press, 2001: 166
(陈 铮,周 飞,王国凡. 材料连接原理. 哈尔滨: 哈尔滨工业大学出版社, 2001: 166)
[22]
Xu N, Ueji R, Morisada Y, Fujii H. Mater Des, 2014; 56: 20
[23]
Yang M, Li M Y, Wang L, Fu Y, Kim J, Weng L. Mater Lett, 2011; 65: 1506
[24]
Chen C Y, Hwang W S. Mater Trans, 2007; 48: 1938
[25]
Chen C Y, Chen H L, Hwang W S. Mater Trans, 2006; 47: 1232
[26]
Jiang H G, Dai J Y, Tong H Y, Ding B Z, Song Q H, Hu Z Q. J Appl Phys, 1993; 74: 6165
[27]
Abbasi M, Taheri K A, Salehi M T. J Alloys Compd, 2001; 319: 233
[28]
Hang C J, Wang C Q, Mayer M, Tian Y H, Zhou Y, Wang H H. Microelectron Reliab, 2008; 48: 416