Please wait a minute...
Acta Metall Sin  2018, Vol. 54 Issue (7): 1068-1076    DOI: 10.11900/0412.1961.2017.00423
Current Issue | Archive | Adv Search |
Microstructure and Mechanical Property of the Welding Joint of TA1/Cu/ X65 Trimetallic Sheets
Min ZHANG(), Erlong MU, Xiaowei WANG, Ting HAN, Hailong LUO
School of Materials Science and Engineering, Xi'an University of Technology, Xi'an 710048, China
Cite this article: 

Min ZHANG, Erlong MU, Xiaowei WANG, Ting HAN, Hailong LUO. Microstructure and Mechanical Property of the Welding Joint of TA1/Cu/ X65 Trimetallic Sheets. Acta Metall Sin, 2018, 54(7): 1068-1076.

Download:  HTML  PDF(7225KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

Titanium and its alloys with fine corrosion resistance and specific tenacity are widely used in the fields of astronautics, chemical industry and so on. While the pipeline steels with low price and good mechanical properties are always used in petroleum industry. For now, composite panels are widely used in petrochemical industry, aerospace engineering and other fields, which can combine the respective features of the dissimilar materials together so as to meet the special requirements and save a lot of rare and precious metals. Previous studies have showed that the joining of titanium and steel suffered from two major challenges: one was the emergence of continuous distributed intermetallics of TiFe and TiFe2 in the weld, which could cause brittle fracture with low strength; the other was the occurrence of residual stresses that were caused by the great differences in thermal properties between titanium and steel. This work is aimed to join the explosion-bonded TA1/Cu/X65 trimetallic sheets (titanium flyer plate with thickness 2 mm, copper intermediate plate 1 mm, and X65 base plate 12 mm) with Cu-based flux-cored wires by the tungsten inert gas (TIG) welding. The microstructure and mechanical properties of welded joint was characterized by using SEM, EDS, TEM, XRD and tensile and microhardness tests. The results indicated that the filler metals for each weld layer have obvious zoning by using solid solution phases and intermetallic compounds. There was about 150 μm width Ti-Cu reaction zone between the Ti weld and transition layer weld. The microstructures of Cu-Ag-Mo-Nb/ER50-6 transition interface were composed of Fe-based and Cu-based solid solution. The intermediate copper played an important role in reducing the high temperature residence time of welded joints so as to reduce the interdiffusion of Ti, Fe element. Consequently, the hard-brittle Ti-Fe intermetallic compounds were partly replaced by Cu-based solid solution and Ti-Cu, Ti-Ag intermetallic compounds with relatively good ductility and toughness. The average tensile strength of the butt joints is 507 MPa at room temperature, mainly of that of X65 was obtained. ERTi-1 weld metal exhibited higher hardness than Cu-Ag-Mo-Nb weld metal, and their microhardness values were 507 and 447 HV100, respectively. In addition, the microhardness in reaction zone presented a slightly drop. The lowest values occurred in ER50-6 weld metal.

Key words:  composite panel      TIG welding      transitional zone      solid solution      intermetallic compound     
Received:  10 October 2017     
ZTFLH:  TG457.19  
Fund: Supported by National Natural Science Foundation of China (No.51274162), Key Laboratory Project of Education Department of Shaanxi Province (No.15JS082) and Service Local Project of Education Department of Shaanxi Province (No.16JF021)

URL: 

https://www.ams.org.cn/EN/10.11900/0412.1961.2017.00423     OR     https://www.ams.org.cn/EN/Y2018/V54/I7/1068

Fig.1  Groove dimensions of the welded plate (The blue rhombus are microhardness test points)
Material C Mn Si Ti Cu Fe O N H S P
TA1 0.015 - - Bal. - 0.023 0.07 0.005 0.001 0.005 0.005
T2 (copper) - - - - Bal. 0.005 - - - 0.005 0.005
X65 0.09 1.32 0.22 - - Bal. - - - 0.005 0.019
Table 1  Chemical compositions of materials applied (mass fraction / %)
Welding material D / mm I / A U / V v / (mmmin-1) Q / (Lmin-1)
ER50-6 1.2 100~120 16~18 150~200 15~20
180~200 20~23 250~350 15~20
Cu-Ag-Mo-Nb 1.2 90~110 16~18 150~250 15~20
ERTi-1 1.2 100~120 14~16 90~110 15~20
Table 2  The welding parameters of TA1/Cu/X65 trimetallic sheets
Fig.2  Microstructures of the welded joint (Figs.2b~j are respectively corresponding to the area marked with numbers 1~9 in black boxes in Fig.2; the points A~T indicated by a black arrow are tested by EDS; WM—welding material)(a) cross-section morphology (b) TA1/Cu-Ag-Mo-Nb/Cu interface (c) TA1/Cu-Ag-Mo-Nb interface(d~g) ERTi-1/Cu-Ag-Mo-Nb interface (h) X65/Cu-Ag-Mo-Nb/Cu interface(i) X65/Cu-Ag-Mo-Nb interface (j) ERTi-1 weld metal
Fig.3  XRD spectrum in the weld of TA1/Cu/X65 trimetallic sheets
Point Ti Cu Fe Ag Mo Nb Possible phase
A 86.44 11.19 1.22 0.72 0.19 0.25 β-Ti(s, s)+Ti2Cu
B 51.90 46.73 - 0.98 0.21 0.18 TiCu
C 84.49 13.44 1.10 0.65 0.32 - β-Ti(s, s)+Ti2Cu
D 67.29 31.88 0.35 0.32 0.05 0.10 Ti2Cu
E 67.29 33.22 0.64 0.42 0.21 0.08 Ti2Cu
F 83.79 13.58 2.10 0.32 0.11 0.10 β-Ti(s, s)+Ti2Cu
G 63.04 30.04 1.62 4.13 0.03 1.14 Ti2Cu+TiCu
H 60.62 32.99 3.85 1.24 1.26 0.04 Ti2Cu
I 39.12 50.01 10.32 0.32 0.13 0.10 Cu0.8Fe0.2Ti
J 7.53 87.41 0.52 4.29 0.16 0.08 Cu(s, s)+TiAg
K 46.75 45.08 4.20 2.31 1.02 0.64 TiCu
L 16.21 82.14 0.62 0.40 0.40 0.23 Cu(s, s)+TiCu4
M 11.19 86.44 1.22 0.72 0.19 0.25 Cu(s, s)+TiCu4
N 14.89 6.94 76.14 0.49 1.14 0.39 Fe(s, s)+TiFe
O 11.74 11.95 66.78 4.21 2.89 2.43 Fe(s, s)+TiCu
P 37.17 48.77 11.43 1.11 0.04 1.49 Cu0.8Fe0.2Ti
Q 1.02 92.36 6.50 0.08 - 0.04 Cu(s, s)
R 15.58 9.21 68.52 6.52 0.12 0.05 Fe(s, s)+TiCu
S 74.32 24.44 1.02 0.13 0.05 0.04 β-Ti(s, s)+Ti2Cu
T 93.99 5.33 0.38 0.21 0.04 0.06 β-Ti(s, s)
Table 3  Chemical compositions of points A~T marked in Fig.2 (atomic fraction / %)
Fig.4  TEM images and corresponding SAED patterns (insets, marked by black circles) of ERTi-1/Cu-Ag-Mo-Nb interface (a) and X65/Cu-Ag-Mo-Nb/Cu interface (b)
Fig.5  Stress-strain curves and fractured samples (inset) for tensile test of the joint
Fig.6  Fracture morphologies of the welded joint (Figs.6b~e are corresponding to the areas marked with letters b~e in a black box in Fig.6a)(a) global view of the fracture (b) ERTi-1 weld metal (c) ERTi-1/Cu-Ag-Mo-Nb reaction zone (d) Cu-Ag-Mo-Nb/ER50-6 (e) ER50-6 weld metal
Fig.7  Microhardness distributions of the welded joint(a) vertical to the ERTi-1, Cu-Ag-Mo-Nb and ER50-6 weld metal (Ti-Cu IMC: Ti2Cu、TiCu、Cu0.8Fe0.2Ti、TiCu4)(b) across the interface of the trimetallic sheet
[1] Banerjee D, Williams J C.Perspectives on titanium science and technology[J]. Acta Mater., 2013, 61: 844
[2] Chu Q L, Zhang M, Li J H, et al.Intermetallics in CP-Ti/X65 bimetallic sheets filled with Cu-based flux-cored wires[J]. Mater. Des., 2016, 90: 299
[3] Lee J G, Hong S J, Lee M K, et al.High strength bonding of titanium to stainless steel using an Ag interlayer[J]. J. Nucl. Mater., 2009, 395: 145
[4] Zhang Y, Sun D Q, Gu X Y, et al.A hybrid joint based on two kinds of bonding mechanisms for titanium alloy and stainless steel by pulsed laser welding[J]. Mater. Lett., 2016, 185: 152
[5] Kahraman N, Gülen? B, Findik F.Joining of titanium/stainless steel by explosive welding and effect on interface[J]. J. Mater. Process. Technol., 2005, 169: 127
[6] Wang T, Zhang B G, Chen G Q, et al.Electron beam welding of Ti-15-3 titanium alloy to 304 stainless steel with copper interlayer sheet[J]. Trans. Nonferrous Met. Soc. China, 2010, 20: 1829
[7] Chu Q L, Zhang M, Li J H, et al.Joining of CP-Ti/Q345 sheets by Cu-based filler metal and effect on interface[J]. J. Mater. Process. Technol., 2015, 225: 67
[8] Van Beek J A, Kodentsov A A, Van loo F J J. Phase equilibria in the Cu-Fe-Ti system at 1123 K[J]. J. Alloys Compd., 1995, 217: 97
[9] Si C Y, Zhou Z F, Zhang Y S.Welding Metallographic Atlas [M]. Beijing: China Machine Press, 1987: 404(斯重遥, 周振丰, 张延生. 焊接金相图谱 [M]. 北京: 机械工业出版社, 1987: 404)
[10] Guo Q W, Wang G S, Guo G C.Common Nonferrous Metal Binary Alloy Phase Portfolio [M]. Beijing: Chemical Industry Press, 2010: 269(郭青蔚, 王桂生, 郭庚辰. 常用有色金属二元合金相图集 [M]. 北京: 化学工业出版社, 2010: 269)
[11] Tomashchuk I, Sallamand P, Jouvard J M.Multiphysical modeling of dissimilar welding via interlayer[J]. J. Mater. Process. Technol., 2011, 211: 1796
[12] Shanmugarajan B, Padmanabham G.Fusion welding studies using laser on Ti-SS dissimilar combination[J]. Opt. Lasers Eng., 2012, 50: 1621
[13] Chen G Q, Zhang B G, Liu W, et al.Influence of electron-beam superposition welding on intermetallic layer of Cu/Ti joint[J]. Trans. Nonferrous Met. Soc. China, 2012, 22: 2416
[14] Lee M K, Lee J G, Choi Y H, et al.Interlayer engineering for dissimilar bonding of titanium to stainless steel[J]. Mater. Lett., 2010, 64: 1105
[15] Wang T, Zhang B G, Chen G Q, et al.High strength electron beam welded titanium-stainless steel joint with V/Cu based composite filler metals[J]. Vacuum, 2013, 94: 41
[16] Shen Q, Xiang H Y, Luo G Q, et al.Microstructure and mechanical properties of TC4/oxygen-free copper joint with silver interlayer prepared by diffusion bonding[J]. Mater. Sci. Eng., 2014, A596: 45
[17] Lee M K, Park J J, Lee G J, et al.Corrosion of Ti-STS dissimilar joints brazed by a Ag interlayer and Ag-Cu-(Pd) alloy fillers[J]. J. Nucl. Mater., 2011, 409: 183
[18] Shiue R K, Wu S K, Shiue J Y.Infrared brazing of Ti-6Al-4V and 17-4 PH stainless steel with (Ni)/Cr barrier layer(s)[J]. Mater. Sci. Eng., 2008, A488: 186
[19] Tomashchuk I, Sallamand P, Andrzejewski H, et al.The formation of intermetallics in dissimilar Ti6Al4V/copper/AISI 316 L electron beam and Nd: YAG laser joints[J]. Intermetallics, 2011, 19: 1466
[20] Bi Z Y, Yang J, Liu H Z, et al.Investigation on the welding process and microstructure and mechanical property of butt joints of TA1/X65 clad plates[J]. Acta Metall. Sin., 2016, 52: 1017(毕宗岳, 杨军, 刘海璋等. TA1/X65复合板焊接工艺及焊缝组织和性能研究[J]. 金属学报, 2016, 52: 1017)
[21] Kundu S, Chatterjee S.Interfacial microstructure and mechanical properties of diffusion-bonded titanium-stainless steel joints using a nickel interlayer[J]. Mater. Sci. Eng., 2006, A425: 107
[22] Ning J, Zhang L J, Jiang G C, et al.Narrow gap multi-pass laser butt welding of explosion welded CP-Ti/Q235B bimetallic sheet by using a copper interlayer[J]. J. Alloys Compd., 2017, 701: 587
[23] Mallesham P, Gokhale A A, Murti V S R. Nature of the interface between AA7072 alloy explosively clad to AA8090 aluminium alloy[J]. J. Mater Sci., 2003, 38: 1869
[24] Dharmendra C, Rao K P, Wilden J, et al.Study on laser welding-brazing of zinc coated steel to aluminum alloy with a zinc based filler[J]. Mater. Sci. Eng., 2011, A528: 1497
[25] Lin S B, Song J L, Yang C L, et al.Brazability of dissimilar metals tungsten inert gas butt welding-brazing between aluminum alloy and stainless steel with Al-Cu filler metal[J]. Mater. Des., 2010, 31: 2637
[26] Ishida K, Gao Y, Nagatsuka K, et al.Microstructures and mechanical properties of friction stir welded lap joints of commercially pure titanium and 304 stainless steel[J]. J. Alloys Compd., 2015, 630: 172
[1] HAN Linzhi, MU Juan, ZHOU Yongkang, ZHU Zhengwang, ZHANG Haifeng. Effect of Heat Treatment Temperature on Microstructure and Mechanical Properties of Ti0.5Zr1.5NbTa0.5Sn0.2 High-Entropy Alloy[J]. 金属学报, 2022, 58(9): 1159-1168.
[2] DING Zongye, HU Qiaodan, LU Wenquan, LI Jianguo. In Situ Study on the Nucleation, Growth Evolution, and Motion Behavior of Hydrogen Bubbles at the Liquid/ Solid Bimetal Interface by Using Synchrotron Radiation X-Ray Imaging Technology[J]. 金属学报, 2022, 58(4): 567-580.
[3] ZHOU Lijun, WEI Song, GUO Jingdong, SUN Fangyuan, WANG Xinwei, TANG Dawei. Investigations on the Thermal Conductivity of Micro-Scale Cu-Sn Intermetallic Compounds Using Femtosecond Laser Time-Domain Thermoreflectance System[J]. 金属学报, 2022, 58(12): 1645-1654.
[4] ZHANG Haijun, QIU Shi, SUN Zhimei, HU Qingmiao, YANG Rui. First-Principles Study on Free Energy and Elastic Properties of Disordered β-Ti1-xNbx Alloy: Comparison Between SQS and CPA[J]. 金属学报, 2020, 56(9): 1304-1312.
[5] CAO Tieshan, ZHAO Jinyi, CHENG Congqian, MENG Xianming, ZHAO Jie. Effect of Cold Deformation and Solid Solution Temperature on σ-phase Precipitation Behavior in HR3C Heat Resistant Steel[J]. 金属学报, 2020, 56(5): 673-682.
[6] Hua JI,Yunlai DENG,Hongyong XU,Weiqiang GUO,Jianfeng DENG,Shitong FAN. The Influence of Welding Line Energy on the Microstructure and Property of CMT Overlap Joint of 5182-Oand HC260YD+Z[J]. 金属学报, 2019, 55(3): 376-388.
[7] Liqun CHEN, Zhengchen QIU, Tao YU. Effect of Ru on the Electronic Structure of the [100](010) Edge Dislocation in NiAl[J]. 金属学报, 2019, 55(2): 223-228.
[8] CAO Lihua, CHEN Yinbo, SHI Qiyuan, YUAN Jie, LIU Zhiquan. Effects of Alloy Elements on the Interfacial Microstructure and Shear Strength of Sn-Ag-Cu Solder[J]. 金属学报, 2019, 55(12): 1606-1614.
[9] HE Xianmei, TONG Liuniu, GAO Cheng, WANG Yichao. Effect of Nd Content on the Structure and Magnetic Properties of Si(111)/Cr/Nd-Co/Cr Thin Films Prepared by Magnetron Sputtering[J]. 金属学报, 2019, 55(10): 1349-1358.
[10] Huijun KANG, Jinling LI, Tongmin WANG, Jingjie GUO. Growth Behavior of Primary Intermetallic Phases and Mechanical Properties for Directionally Solidified Al-Mn-Be Alloy[J]. 金属学报, 2018, 54(5): 809-823.
[11] Chuang DONG, Dandan DONG, Qing WANG. Chemical Units in Solid Solutions andAlloy Composition Design[J]. 金属学报, 2018, 54(2): 293-300.
[12] Yinhui ZHANG, Qiang FENG. Effects of W on Creep Behaviors of Novel Nb-Bearing Austenitic Heat-Resistant Cast Steels at 1000 ℃[J]. 金属学报, 2017, 53(9): 1025-1037.
[13] Ning ZHAO,Jianfeng DENG,Yi ZHONG,Luqiao YIN. Evolution of Interfacial Intermetallic Compounds in Ni/Sn-xCu/Ni Micro Solder Joints Under Thermomigration During Soldering[J]. 金属学报, 2017, 53(7): 861-868.
[14] Hongwei ZHANG,Xuezhi QIN,Xiaowu LI,Lanzhang ZHOU. Incipient Melting Behavior and Its Influences on the Mechanical Properties of a Directionally Solidified Ni-Based Superalloy with High Boron Content[J]. 金属学报, 2017, 53(6): 684-694.
[15] Zhijie ZHANG,Mingliang HUANG. Liquid-Solid Electromigration Behavior of Cu/Sn-52In/Cu Micro-Interconnect[J]. 金属学报, 2017, 53(5): 592-600.
No Suggested Reading articles found!