Effects of V on the Microstructure Evolution and Hardness Enhancement of Ti2AlNb Alloy
LIU Ziru1, GUO Qianying1(), ZHANG Hongyu2, LIU Yongchang1()
1 State Key Laboratory of High Performance Roll Materials and Composite Forming, School of Materials Science and Engineering, Tianjin University, Tianjin 300354, China 2 New Materials Computing Research Center, Zhejiang Laboratory, Hangzhou 311100, China
Cite this article:
LIU Ziru, GUO Qianying, ZHANG Hongyu, LIU Yongchang. Effects of V on the Microstructure Evolution and Hardness Enhancement of Ti2AlNb Alloy. Acta Metall Sin, 2025, 61(6): 848-856.
Ti2AlNb-based alloys, as emerging lightweight high-temperature structural materials, have shown great potential for aerospace applications owing to their outstanding creep resistance, strong plasticity, and impressive high-temperature oxidation resistance. However, the material has yet to see widespread use owing to its poor formability and processability. Compared to traditional melting and forging methods, powder metallurgy has proven to be an effective method for preparing this alloy with a required shape, thereby circumventing phase transformation during hot working. The properties of Ti2AlNb-based alloy can be enhanced by adding stabilized elements to the B2 or α2 phase. Among these metallic elements, V has been demonstrated to effectively increase the ductility and high-temperature strength of Ti2AlNb-based alloys. However, the mechanism of the V addition's effect on the microstructure and properties of Ti2AlNb-based alloys during aging treatment has not been systematically clarified. Therefore, investigating the influence of powder sintering and post-heat treatment on the microstructure and properties of Ti-22Al-25Nb-1V alloys is crucial for accelerating their industrialization process. This investigation forms the basis of this work. A detailed study on the role of V in the microstructure and deformation responses of the Ti2AlNb alloy was performed. This involved preparing V-added and V-free Ti-22Al-25Nb alloys via spark plasma sintering. Then, the sintered alloys were solution treated at 1300 oC for 4 h and subsequently aged at temperatures from 800 oC to 1050 oC for 2 h for microstructure modification. The detailed microstructure of the alloys was analyzed using X-ray diffraction and electron microscopy. The results revealed that by adding V, the volume fraction of the residual α2 phase improves. The microhardness of the V-doped alloys is significantly enhanced compared to the undoped alloys and reached a maximum value of 503 HV at an aging temperature of 850 oC. This α2 phase pins the grain boundary during heat treatment, resulting in an alloy with a refined grain size. Additionally, V additions can inhibit the B2 + α2 → O transition, promoting a finer O/α2 phase precipitate and higher hardness. Furthermore, microstructural analysis proved that the segregation of V and Nb in the B2 phase will cause the “curved” structure, including Nb- and V-rich B2 and Nb- and V-lean α2 phases. The partial replacement of Nb by V reduced the lattice parameter in the B2 phase, which further improves the hardness of this alloy.
Table 1 Chemical compositions of the sintered Ti-22Al-25Nb and Ti-22Al-25Nb-1V samples
Fig.1 XRD spectra of Ti-22Al-25Nb and Ti-22Al-25Nb-1V alloys after solution treatment at 1300 ºC
Fig.2 XRD spectra of Ti-22Al-25Nb (a) and Ti-22Al-25Nb-1V (b) alloys after solution treatment at 1300 ºC and aging at different temperatures
Fig.3 SEM images of the Ti-22Al-25Nb alloy after solution treatment at 1300 ºC and aging at 800 ºC (a), 850 ºC (b), 900 ºC (c), 950 ºC (d), 1000 ºC (e), and 1050 ºC (f)
Fig.4 SEM images of the Ti-22Al-25Nb-1V alloys after solution treatment at 1300 ºC and aging at 800 ºC (a), 850 ºC (b), 900 ºC (c), 950 ºC (d), 1000 ºC (e), and 1050 ºC (f)
Fig.5 Vickers hardnesses of the Ti-22Al-25Nb and Ti-22Al-25Nb-1V alloys after solution treatment at 1300 ºC and aging at 800-1050 ºC
Temperature / oC
Alloy
B2 phase
O phase
α2 phase
800
Ti-22Al-25Nb
18.33
81.67
-
Ti-22Al-25Nb-1V
21.33
73.68
4.99
850
Ti-22Al-25Nb
27.93
72.07
-
Ti-22Al-25Nb-1V
38.80
51.22
9.98
900
Ti-22Al-25Nb
42.03
57.97
-
Ti-22Al-25Nb-1V
49.62
31.08
19.30
950
Ti-22Al-25Nb
71.81
14.71
13.48
Ti-22Al-25Nb-1V
74.48
-
25.52
1000
Ti-22Al-25Nb
81.53
-
18.47
Ti-22Al-25Nb-1V
85.03
-
14.97
1050
Ti-22Al-25Nb
84.04
-
15.96
Ti-22Al-25Nb-1V
80.91
-
19.09
Table 2 Volume fractions of B2, O, and α2 phases of the Ti-22Al-25Nb and Ti-22Al-25Nb-1V alloys after solution treatment at 1300 oC and aging at different temperatures
Fig.6 B2 phase grain sizes of the Ti-22Al-25Nb and Ti-22Al-25Nb-1V alloys after solution treatment at 1300 ºC and aging at different temperatures
Fig.7 Widths of the precipitated phase of the Ti-22Al-25Nb and Ti-22Al-25Nb-1V alloys after solution treatment at 1300 ºC and aging at different temperatures
Fig.8 Phase map of the Ti-22Al-25Nb-1V alloy after solution treatment at 1300 ºC and aging at 900 ºC
Fig.9 SEM backscattered electron (BSE) image (a) and corresponding linear scan analyses alone the line in Fig.9a (b) of the Ti-22Al-25Nb-1V alloy after solution treatment at 1300 ºC and aging at 900 ºC
Fig.10 TEM images of Ti-22Al-25Nb (a) and Ti-22Al-25Nb-1V (b) alloys after solution treatment at 1300 ºC and aging at 850 ºC (Inset in Fig.11b shows the SAED pattern of region A)
Fig.11 TEM bright field image (a) and corresponding SAED patterns of regions A (b) and B (c) in Fig.11a showing the discontinuous microstructure for the Ti-22Al-25Nb alloy after solution treatment at 1300 ºC and aging at 850 ºC
Fig.12 TEM image (a) and corresponding SAED patterns of regions A (b) and B (c) in Fig.12a showing the curved microstructure for the Ti-22Al-25Nb-1V alloy after solution treatment at 1300 ºC and aging at 850 ºC
Temperature / oC
Alloy
a / nm
d(110) / nm
d(200) / nm
d(211) / nm
800
Ti-22Al-25Nb
0.32518
0.22994
0.16259
0.13275
Ti-22Al-25Nb-1V
0.32455
0.22949
0.16227
0.13250
850
Ti-22Al-25Nb
0.32512
0.22989
0.16256
0.13273
Ti-22Al-25Nb-1V
0.32455
0.22949
0.16227
0.13250
900
Ti-22Al-25Nb
0.32506
0.22985
0.16253
0.13271
Ti-22Al-25Nb-1V
0.32398
0.22909
0.16199
0.13226
950
Ti-22Al-25Nb
0.32428
0.22930
0.16214
0.13239
Ti-22Al-25Nb-1V
0.32368
0.22888
0.16184
0.13214
1000
Ti-22Al-25Nb
0.32413
0.22919
0.16206
0.13232
Ti-22Al-25Nb-1V
0.32365
0.22886
0.16182
0.13213
1050
Ti-22Al-25Nb
0.32446
0.22943
0.16223
0.13246
Ti-22Al-25Nb-1V
0.32398
0.22909
0.16199
0.13226
Table 3 Lattice constarts (a) and interplanar spacings (d) of the B2 phase in the alloy with different aging temperatures
1
Mikhaylovskaya A V, Mosleh A O, Mestre-Rinn P, et al. High-strength titanium-based alloy for low-temperature superplastic forming [J]. Metall. Mater. Trans., 2021, 52A: 293
2
Zhang Y, Lee Y J, Chang S, et al. Microstructural modulation of TiAl alloys for controlling ultra-precision machinability [J]. Int. J. Mach. Tools Manuf., 2022, 174: 103851
3
Banerjee D, Gogia A K, Nandi T K, et al. A new ordered orthorhombic phase in a Ti3Al-Nb alloy [J]. Acta Metall., 1988, 36: 871
4
Huang Y, Liu Y C, Li C, et al. Microstructure evolution and phase transformations in Ti-22Al-25Nb alloys tailored by super-transus solution treatment [J]. Vacuum, 2019, 161: 209
5
Zhang Y R, Cai Q, Liu Y C. Formation of diverse B2 + O structure and hardness of Mo-modified Ti-22Al-25Nb alloys upon cooling [J]. Vacuum, 2019, 165: 199
6
Zhang H Y, Zhang Y R, Liang H Y, et al. Effect of the primary O phase on thermal deformation behavior of a Ti2AlNb-based alloy [J]. J. Alloys Compd., 2020, 846: 156458
7
Zheng Y P, Zeng W D, Li D, et al. Quasi cleavage fracture of the bimodal size lamellar O phase microstructure of a Ti2AlNb-based alloy [J]. J. Alloys Compd., 2019, 799: 267
8
Feng A H, Chen Q, Wang J, et al. Thermal stability of microstructures in low-density Ti2AlNb-based alloy hot rolled plate [J]. Acta Metall. Sin., 2023, 59: 777
Valkov S, Bezdushnyi R, Petrov P. Synthesis, structure and mechanical properties of Ti-Al-Nb coatings formed by electron beam additive technique [J]. Vacuum, 2018, 156: 140
10
Yang R, Hao Y L, Obbard E G, et al. Orthorhombic phase transformations in titanium alloys and their applications [J]. Acta Metall. Sin., 2010, 46: 1443
doi: 10.3724/SP.J.1037.2010.00483
杨 锐, 郝玉琳, Obbard E G 等. 钛合金中的正交相变及其应用 [J]. 金属学报, 2010, 46: 1443
11
Dey S R, Roy S, Suwas S, et al. Annealing response of the intermetallic alloy Ti-22Al-25Nb [J]. Intermetallics, 2010, 18: 1122
12
Wang W, Zeng W D, Li D, et al. Microstructural evolution and tensile behavior of Ti2AlNb alloys based α2-phase decomposition [J]. Mater. Sci. Eng., 2016, A662: 120
13
Zhang H Y, Li C, Ma Z Q, et al. Morphology and quantitative analysis of O phase during heat treatment of hot-deformed Ti2AlNb-based alloy [J]. Int. J. Miner. Metall. Mater., 2018, 25: 1191
14
Niu H Z, Chen Y F, Zhang D L, et al. Fabrication of a powder metallurgy Ti2AlNb-based alloy by spark plasma sintering and associated microstructure optimization [J]. Mater. Des., 2016, 89: 823
15
Zhang H Y, Yan N, Liang H Y, et al. Phase transformation and microstructure control of Ti2AlNb-based alloys: A review [J]. J. Mater. Sci. Technol., 2021, 80: 203
16
Goyal K, Sardana N. Mechanical properties of the Ti2AlNb intermetallic: A review [J]. Trans. Indian Inst. Met., 2021, 74: 1839
17
Zheng Y P, Zeng W D, Li D, et al. Orthorhombic precipitate variant selection in a Ti2AlNb based alloy [J]. Mater. Des., 2018, 158: 46
18
Bu Z Q, Zhang Y G, Yang L, et al. Effect of cooling rate on phase transformation in Ti2AlNb alloy [J]. J. Alloys Compd., 2022, 893: 162364
19
Liu X Z, Wang J, Li Y M, et al. Densification mechanism of Ti-Al-Nb alloys pressurelessly sintered from Al-Nb master alloy powder for cost-effective manufacturing [J]. J. Alloys Compd., 2023, 936: 168307
20
Raynova S, Yang F, Bolzoni L. Mechanical behaviour of induction sintered blended elemental powder metallurgy Ti alloys [J]. Mater. Sci. Eng., 2021, A799: 140157
21
Fang Z Z, Paramore J D, Sun P, et al. Powder metallurgy of titanium—Past, present, and future [J]. Int. Mater. Rev., 2018, 63: 407
22
Yang J L, Wang G F, Jiao X Y, et al. High-temperature deformation behavior of the extruded Ti-22Al-25Nb alloy fabricated by powder metallurgy [J]. Mater. Charact., 2018, 137: 170
23
Sim K H, Wang G F, Kim T J, et al. Fabrication of a high strength and ductility Ti-22Al-25Nb alloy from high energy ball-milled powder by spark plasma sintering [J]. J. Alloys Compd., 2018, 741: 1112
24
Sim K H, Wang G F, Son R C, et al. Influence of mechanical alloying on the microstructure and mechanical properties of powder metallurgy Ti2AlNb-based alloy [J]. Powder Technol., 2017, 317: 133
25
Emura S, Tsuzaki K, Tsuchiya K. Improvement of room temperature ductility for Mo and Fe modified Ti2AlNb alloy [J]. Mater. Sci. Eng., 2010, A528: 355
26
Tang F, Nakazawa S, Hagiwara M. The effect of quaternary additions on the microstructures and mechanical properties of orthorhombic Ti2AlNb-based alloys [J]. Mater. Sci. Eng., 2002, A329-331: 492
27
Cheng F, Wang H M, Yang J W, et al. Deformation kinking in duplex titanium alloy with widmannstatten laths under high strain rates [J]. Mater. Lett., 2023, 333: 133591
28
Liu Z R. Ageing precipitation behavior and mechanical properties of Ti-22Al-25Nb-1Valloys by powder metallurgy [D]. Tianjin: Tianjin University, 2023
Sadi F A, Servant C. On the B2 → O phase transformation in Ti-Al-Nb alloys [J]. Mater. Sci. Eng., 2003, A346: 19
30
Zong Y Y, Wang J W, Shao B, et al. Mechanism and morphology evolution of the O phase transformation in Ti-22Al-25Nb alloy [J]. Mater. Sci. Technol., 2021, 89: 97
31
Zhang Y F, Tian S W, Jiang H T, et al. Research on hot deformation behavior of Mo‐containing Ti2AlNb‐based alloy [J]. Adv. Eng. Mater., 2021, 23: 2100449
32
Shao B, Shan D B, Guo B, et al. Plastic deformation mechanism and interaction of B2, α2, and O phases in Ti-22Al-25Nb alloy at room temperature [J]. Int. J. Plast., 2019, 113: 18
33
He Y S, Hu R, Luo W Z, et al. Microstructural evolution and creep deformation behavior of novel Ti-22Al-25Nb-1Mo-1V-1Zr-0.2Si (at.%) orthorhombic alloy [J]. Trans. Nonferrous Met. Soc. China, 2019, 29: 313
34
Fu Y Q, Cui Z S. Effects of plastic deformation and aging treatment on phase precipitation in Ti2AlNb Alloy [J]. J. Mater. Eng. Perform., 2022, 31: 2633