Please wait a minute...
金属学报  2026, Vol. 62 Issue (7): 1207-1227    DOI: 10.11900/0412.1961.2025.00354
  综述 本期目录 | 过刊浏览 |
超高强度钢析出相调控与强化机理研究现状及发展趋势
张朝磊(), 潘晓坤, 高军恒, 吴宏辉, 毛新平
北京科技大学 碳中和研究院 北京 100083
Research Status and Development Trend of Precipitation Phase Regulation and Strengthening Mechanism in Ultra-High Strength Steel
ZHANG Chaolei(), PAN Xiaokun, GAO Junheng, WU Honghui, MAO Xinping
Institute for Carbon Neutrality, University of Science and Technology Beijing, Beijing 100083, China
引用本文:

张朝磊, 潘晓坤, 高军恒, 吴宏辉, 毛新平. 超高强度钢析出相调控与强化机理研究现状及发展趋势[J]. 金属学报, 2026, 62(7): 1207-1227.
Chaolei ZHANG, Xiaokun PAN, Junheng GAO, Honghui WU, Xinping MAO. Research Status and Development Trend of Precipitation Phase Regulation and Strengthening Mechanism in Ultra-High Strength Steel[J]. Acta Metall Sin, 2026, 62(7): 1207-1227.

全文: PDF(3807 KB)   HTML
摘要: 

作为航空、航天及重大装备的关键结构材料,超高强度钢的轻量化与高性能化是相关领域发展的核心需求。然而,传统超高强度钢长期面临高强度与高韧性、良好焊接性与耐蚀性难以协同,以及高合金成本制约其广泛应用等问题。为应对上述问题,本文系统梳理了低合金超高强度钢、二次硬化钢、马氏体时效钢及沉淀硬化不锈钢等传统超高强度钢的发展历程、成分、组织和性能特征,进而重点综述了通过复合纳米析出相调控和多相复合组织设计两类路径开发的新型超高强度钢的研究进展,特别探讨了“混杂化(hybrid)”设计新理念在突破传统钢种界限、融合多相强化机制,以及研制低成本、高性能、易焊接“全能型”超高强度钢方面的潜力与初步实践。详细阐述了超高强度钢中析出相演变规律和强化机理研究现状。最后,对超高强度钢的未来发展方向,特别是在复杂析出相协同调控、高温稳定性及产业化应用等方面的挑战与机遇进行了展望。

关键词 : 超高强度钢,  碳化物,  金属间化合物,  强化机理    
Abstract:

As a key structural material for aviation, aerospace, and major equipment, the lightweight and high-performance development of ultra-high strength (UHS) steel is essential for the advancement of related fields. However, traditional UHS steels have long faced critical challenges: the difficulty in achieving a synergistic combination of high strength, high toughness, good weldability, and corrosion resistance, along with the constraint of high alloy costs that limit their widespread application. To address these issues, we systematically review the development history, composition, microstructure, and performance characteristics of traditional UHS steels, including low-alloy UHS, secondary hardening, maraging, and precipitation-hardening stainless steels. We also review the research progress in developing novel UHS steels through two main pathways: the regulation of composite nanoprecipitates and the design of multiphase composite microstructures. Special attention is paid to exploring the potential and preliminary practices of the “hybrid” design concept, which breaks the boundaries of traditional steel classifications and integrates multiple strengthening mechanisms to develop cost-effective, high-performance, and easily weldable “all-round” UHS steels. The current research status regarding the evolution laws of precipitates and strengthening mechanisms in UHS steels is detailed. Finally, the future development directions of UHS steels are proposed, particularly regarding the synergistic control of complex precipitates, high-temperature stability, and industrial application.

Key words: ultra-high strength steel    carbide    intermetallic compound    strengthening mechanism
收稿日期: 2025-11-03     
ZTFLH:  TG142.1  
基金资助:国家自然科学基金项目(52574422)
通讯作者: 张朝磊,zhangchaolei@ustb.edu.cn,主要从事高性能特殊钢材料及其应用研究
Corresponding author: ZHANG Chaolei, professor, Tel: 13581677127, E-mail: zhangchaolei@ustb.edu.cn
作者简介: 张朝磊,男,1984年生,教授,博士
图1  典型超高强度钢的屈服强度与断裂韧性的关系[1~15]

Steel

Mass fraction / %

UTS

MPa

YS

MPa

Impact energy / JRef.
CMnSiCrNiMoV
AISI43400.38-0.430.60-0.800.20-0.350.70-0.901.65-2.000.20-0.30-1802152825[20]
300M0.41-0.460.65-0.901.45-1.800.65-0.951.60-2.000.30-0.40≥ 0.051890160528[17]
30CrMnSiNi2A0.27-0.341.00-1.301.00-1.200.90-1.201.40-1.80--1720140075[21]
D6AC0.44-0.490.60-0.900.15-0.350.90-1.200.40-0.700.90-1.100.05-0.152080184013[22]
表1  典型低合金超高强度钢的化学成分及力学性能[17,20~22]

Steel type

Steel grade

Mass fraction / %

UTS

MPa

YS

MPa

Impact energy / J

Ref.

CMnCoCrNiMoTiOther
Secondary hardeningAF14100.1614.014.02.110.11.0--1655152061[24]
ultra-high strength steelAerMet1000.2313.513.53.011.21.2--1993176041[9]
HY1800.107.57.51.89.51.0--1413134585[30]
Maraging steel18Ni(250)-8.98.9-18.34.70.6-1854181935[31]
T250----183.01.50.1Al1860150058[27]
W250----19-1.24.5W + 0.1Al1800178025[32]
Precipitation-hardeningPH13-80.03--12.67.91.7-1.0Al1551144841[28]
(PH) ultra-highCustom4650.02--12.49.840.70.24-10801039150[29]
strength stainless steelFerriumS530.21-13.09.04.81.50.021.0W1986155118[28]
表2  典型中高合金超高强钢的化学成分及力学性能[9,24,27~32]
Steel typeChemical compositionMicrostructureKey processPerformance characteristicDrawbackRef.

Low-alloy ultra-high strength steel

C 0.25%-0.60%, Cr 5%, Si 5%, Ni 5%

Tempered martensite + fine dispersed carbides

Quenching + low temperature tempering, or isothermal quenching

Low cost and simple production process

Insufficient toughness, poor corrosion resistance and weldability

[35]

Secondary hardening ultra-high strength steelC 0.10%-0.40%, Cr 5%-25%, Ni 5%-25%, Co 5%-25%Tempered martensite (+ retained austenite) + carbides

Quenching + tempering

Excellent fatigue resistance and stress corrosion cracking resistance

High cost, prone to segregation

[36]

Maraging steel

C 0.1%, Ni 20%, Co 20%, Mo 20%Low-carbon Fe-Ni martensitic matrix + intermetallic compounds (such as Ni3Ti and Ni3Mo)

Solution treatment + aging

Good cold formability, simple heat treatment, and excellent weldabilitySensitive to compositional fluctuations, high cost

[37]

PH ultra-high strength stainless steel

C 0.25%, Cr 12%, Ni 12%

Tempered martensite + intermetallic compounds (such as NiAl, Ni3Ti, and Laves phase)

Solution treatment + aging

Good weldability, easy machinability, and excellent corrosion resistance

High Cr and Ni contents, high cost

[1]

表3  传统超高强度钢的合金成分、显微组织、关键工艺、性能特征及缺点[1,35~37]
图2  新型马氏体时效钢的力学性能及析出相表征[38]
图3  高位错密度诱导大塑性变形-配分超高强度钢的微观组织形貌、观察方向及拉伸曲线[50]
Steel typeChemical compositionMicrostructureKey processMechanical propertyDrawbackRef.

Novel maraging steel

0.08%C-18%Ni-3%Al-4%Mo-0.8%NbMartensite + high density Ni(Al, Fe) coherent nano-precipitates

Solution treatment + aging

UTS = 2200 MPa, EL = 8%High Ni content and high alloy cost

[38]

Ultra-high strength steel with composite nano-precipitates

C 0.1%,Ni 10%, Cr 10%, Co 10%

Martensite + composite nano-precipitates (NiAl, Laves phase, MC carbide, Cu particles)

Solution treatment + aging

UTS 1800 MPa, EL 8%

Precipitate composition and sequence sensitive to chemical composition

[41,46]

Ultra-high strength steel with multiphase composite microstructure

C 0.25%-0.6%,Mn 5%, Cr 5%

Martensite (+ bainite) + retained austenite + small carbideQuenching + partitioning (+ tempering)UTS = 2000 MPa, EL = 10%Poor weldability, microstructure sensitive to composition

[51,52]

Nanostructured bainitic steel

C 0.3%,Ni 10%, Si 10%, Mn 10%

Bainitic ferrite lath (20-40 nm) + retained austenite (volume fraction 20%)

Bainite isothermal transformation + tempering/partitioning/cryogenic treatment

UTS = 2500 MPa, EL 8%

Long isothermal transformation period, poor weldability

[53]

Ultra-high strength steel subjected to severe plastic deformation and partitioning induced by high dislocation density

0.47%C-10%Mn-2%Al-0.7%V

High density dislocation martensite + metastable austenite

Cold rolling + low temperature tempering

YS 2200 MPa, EL 16%

Complex processing, deformation parameters and heat treatment need stir control

[50]

表4  新型超高强度钢的化学成分、显微组织、关键工艺和力学性能及缺点[38,41,46,50~53]
图4  三种典型增材制造工艺示意图:激光粉末床熔融[56]、激光直接能量沉积[58]及电弧增材制造[59]
图5  “混杂化(hybrid)”设计理念
图6  超高强度钢中典型碳化物形貌[76~78]
PrecipitatePhaseCrystal structureChemical compositionTypical orientation relationshipShape

Carbide

MCfcc(Ti, Mo, Nb, V)C(100) MC//(100) α, [010] MC//[011] αDisk-like

M2C

(η-carbide)

hcp(Mo, Cr, V, Mn)2C(110) η //(101) α, [001] η //[100] αIrregular
ε-carbidehcpFe2.4C[21¯1¯0] ε //[11¯1] αNeedle-like
M3COrthorhombic structure(Fe, Mn, Cr)3C(001)M3C//(1¯12) α, [100]M3C//[01¯1] αNeedle-like
M7C3hcp(Cr, Fe)7C3-Fine and dispersed
M23C6fcc(Cr, Fe, Mo)23C6(100)M23C6//(100) α, [010]M23C6//[010] αChain-like
M6Cfcc

(Ni, Co)6C,

(Fe, W, Mo)6C

(001)M6C/(011) α, [110]M6C//[111] αCubic

Intermetallic

compound and

Cubcc, 9R, fccCu, Fe, Al, Ni, Mn(110)9R//(111) α, [114¯]9R//[01¯1] αSpherical, elongated
nanoclusterNi3Mhcp, fcc,(Ni, Fe, Co)3(Ti, Mo, Al)(010)Ni3Mo//(011)B, [100]Ni3Mo//[111¯]BDisk-like, rod-like
NiAlB2, bccNi, Al, Mn, Fe, Cu{001}NiAl//{001}B, 110NiAl//110BSpherical, elongated

Fe2M

(Laves phase)

hcpFe2(Mo, Nb, W)(011¯2)Fe2W//(001) α, [011¯1¯]Fe2W//[11¯0] αSpherical, irregular
表5  超高强度钢中典型碳化物、金属间化合物及纳米团簇特征[82~89]
图7  新型超高强度钢中典型复合析出相的析出机制[91,92,94,95]
图8  超高强度钢中NiAl和M2C复合析出结构、M2C、NiAl的TEM分析及NiAl与M2C的复合析出机制[97,99]
[1] Luo H W, Shen G H. Progress and perspective of ultra-high strength steels having high toughness [J]. Acta Metall. Sin., 2020, 56: 494
doi: 10.11900/0412.1961.2019.00328
[1] 罗海文, 沈国慧. 超高强高韧化钢的研究进展和展望 [J]. 金属学报, 2020, 56: 494
doi: 10.11900/0412.1961.2019.00328
[2] Li H F, Wang S G, Zhang P, et al. Crack propagation mechanisms of AISI 4340 steels with different strength and toughness [J]. Mater. Sci. Eng., 2018, A729: 130
[3] Liu F G, Lin X, Song M H, et al. Effect of tempering temperature on microstructure and mechanical properties of laser solid formed 300M steel [J]. J. Alloys Compd., 2016, 689: 225
doi: 10.1016/j.jallcom.2016.07.276
[4] Zhang Y P, Zhan D P, Qi X W, et al. Effect of solid-solution temperature on the microstructure and properties of ultra-high-strength ferrium S53® steel [J]. Mater. Sci. Eng., 2018, A730: 41
[5] Daymond B T, Binot N, Schmidt M L, et al. Development of custom 465® corrosion-resisting steel for landing gear applications [J]. J. Mater. Eng. Perform., 2016, 25: 1539
doi: 10.1007/s11665-015-1830-5
[6] Li Y C, Yan W, Cotton J D, et al. A new 1.9 GPa maraging stainless steel strengthened by multiple precipitating species [J]. Mater. Des., 2015, 82: 56
doi: 10.1016/j.matdes.2015.05.042
[7] Maloney J L, Garrison W M. The effect of sulfide type on the fracture behavior of HY180 steel [J]. Acta Mater., 2005, 53: 533
doi: 10.1016/j.actamat.2004.09.041
[8] Li Y F, Cheng X, Liu D, et al. Influence of last stage heat treatment on microstructure and mechanical properties of laser additive manufactured AF1410 steel [J]. Mater. Sci. Eng., 2018, A713: 75
[9] Manigandan K, Srivatsan T S, Tammana D, et al. Influence of microstructure on strain-controlled fatigue and fracture behavior of ultra high strength alloy steel AerMet 100 [J]. Mater. Sci. Eng., 2014, A601: 29
[10] Prasad N E, Wanhill R J H. Aerospace Materials and Material Technologies [M]. Singapore: Springer, 2017: 173
[11] Morris J W. Making steel strong and cheap [J]. Nat. Mater., 2017, 16: 787
doi: 10.1038/nmat4949 pmid: 28748963
[12] He Y, Yang K, Kong F Y, et al. Mechanical properties of ultra-high-strength 18Ni cobalt-free maraging steel [J]. Acta Metall. Sin., 2002, 38: 278
[12] 何 毅, 杨 柯, 孔凡亚 等. 超高强度18Ni无钴马氏体时效钢的力学性能 [J]. 金属学报, 2002, 38: 278
[13] Gao Y H, Liu S Z, Hu X B, et al. A novel low cost 2000 MPa grade ultra-high strength steel with balanced strength and toughness [J]. Mater. Sci. Eng., 2019, A759: 298
[14] Liu Z B, Yang Z, Wang X H, et al. Enhanced strength-ductility synergy in a new 2.2 GPa grade ultra-high strength stainless steel with balanced fracture toughness: Elucidating the role of duplex aging treatment [J]. J. Alloys Compd., 2022, 928: 167135
doi: 10.1016/j.jallcom.2022.167135
[15] Niu G, Zurob H S, Misra R D K, et al. Superior fracture toughness in a high-strength austenitic steel with heterogeneous lamellar microstructure [J]. Acta Mater., 2022, 226: 117642
doi: 10.1016/j.actamat.2022.117642
[16] Leo D W, Varadarajan A S. Simulation of surface milling of hardened AISI 4340 steel with minimal fluid application using artificial neural network [J]. Adv. Prod. Eng. Manag., 2012, 1: 51
[17] Kasana, S S, Sharma S, Pandey O P. Influence of heat treatment (routes) on the microstructure and mechanical properties of 300M ultra high strength steel [J]. Arch. Civ. Mech. Eng., 2022, 22: 126
doi: 10.1007/s43452-022-00439-z
[18] Feng D Y, Liu S C, Wang S L, et al. Effect of heat treatment on microstructure and mechanical properties of electron beam welding joint of 30CrMnSiNi2A steel [J]. Mater. Rep., 2025, 39(14): 132
[18] 冯殿远, 刘诗超, 王善林 等. 热处理对30CrMnSiNi2A钢电子束焊接头组织和性能的影响 [J]. 材料导报, 2025, 39(14): 132
[19] Chen D M, Kang M K, Tan R B. Fatigue properties of meta-bainite in steel 40CrMnSiMoVA [J]. Acta Metall. Sin., 1991, 27: A458
[19] 陈大明, 康沫狂, 谭若兵. 40CrMnSiMoVA钢准贝氏体的疲劳性能 [J]. 金属学报, 1991, 27: A458
[20] Tikhe O, Doiphode P, Nichul U, et al. Development of optimized mechanical properties of AISI 4340 steel: Role of quenching and partitioning process [J]. Met. Mater. Int., 2023, 29: 2216
doi: 10.1007/s12540-022-01375-6
[21] Liu X M, Hua F, Liu R, et al. Effect of heat treatment on the mechanical properties of steel 30CrMnSiNi2A [J]. Iron Steel, 2003, 38(1): 43
[21] 刘宪民, 花 峰, 刘 蕤 等. 热处理对30CrMnSiNi2A钢力学性能的影响 [J]. 钢铁, 2003, 38(1): 43
[22] Khodamorad A, Hassan S, Shahram K. Bainite-martensite microstructure in D6AC steel effect of bainite morphology on mechanical properties of the mixed [J]. J. Mater. Sci. Technol., 2012, 28: 336
doi: 10.1016/S1005-0302(12)60065-6
[23] Maloney J L, Garrison W M. The effect of sulfide type on the fracture behavior of HY180 steel [J]. Acta Mater., 2005, 53: 533
doi: 10.1016/j.actamat.2004.09.041
[24] Handerhan K J, Garrison W M, Moody N R. A comparison of the fracture behavior of two heats of the secondary hardening steel AF1410 [J]. Metall. Trans., 1989, 20A: 105
[25] Thomas R L S, Li D M, Gangloff R P, et al. Trap-governed hydrogen diffusivity and uptake capacity in ultrahigh-strength AERMET100 steel [J]. Metall. Mater. Trans., 2002, 33A: 1991
[26] Morikawa H, Komatsu H, Tanino M. Effect of chromium upon co‐herency between M2C precipitates and α-iron matrix in 0.1C-10Ni-8Co-lMo-Cr steels [J]. J. Electron. Microsc., 1973, 22: 99
[27] Li K, Shan J G, Wang C X, et al. Strength and toughness of T250 maraging steel joint hybrid-treated with laser welding and aging [J]. Acta Metall. Sin., 2015, 51: 904
doi: 10.11900/0412.1961.2014.00635
[27] 李 坤, 单际国, 王春旭 等. T250马氏体时效钢激光焊接-时效处理接头的强韧性 [J]. 金属学报, 2015, 51: 904
[28] Liu Z B, Liang J X, Su J, et al. Research and application progress in ultra-high strength stainless steel [J]. Acta Metall. Sin., 2020, 56: 549
[28] 刘振宝, 梁剑雄, 苏 杰 等. 高强度不锈钢的研究及发展现状 [J]. 金属学报, 2020, 56: 549
doi: 10.11900/0412.1961.2019.00453
[29] Anoop C R, Prakash A, Narayana Murty S V S, et al. Origin of low temperature toughness in a 12Cr-10Ni martensitic precipitation hardenable stainless steel [J]. Mater. Sci. Eng., 2018, A709: 1
[30] Bray J W, Maloney J L, Raghavan K S, et al. A comparison of the fracture behavior of two commercially produced heats of HY180 steel differing in sulfide type [J]. Metall. Trans., 1991, 22A: 2277
[31] Luo H, Yin Z D, Zhu J C, et al. Influence of grain size on mechanical properties of 18Ni maraging steel [J]. Mater. Sci. Technol., 2000, 8(1): 59
[31] 罗 鸿, 尹钟大, 朱景川 等. 晶粒尺寸对18Ni马氏体时效钢力学性能的影响 [J]. 材料科学与工艺, 2000, 8(1): 59
[32] Kim Y G, Kim G S, Lee C S, et al. Microstructure and mechanical properties of a cobalt-free tungsten-bearing maraging steel [J]. Mater. Sci. Eng., 1986, 79: 133
[33] Yang W Y. Investigation on strength-toughness mechanism of low nickel, cobalt free maraging steel [D]. Taiyuan: North University of China, 2009
[33] 杨维宇. 低Ni无Co马氏体时效钢强韧化研究 [D]. 太原: 中北大学, 2009
[34] Kuehmann C, Tufts B, Trester P. Computational design for ultra high-strength alloy [J]. AMP Tech. Artic., 2008, 166: 37
[35] Niu Y E, Zhao P P, Li N, et al. Research status and application of ultra-high strength steel at home and abroad [J]. J. Ordnance Equip. Eng., 2021, 42(7): 274
[35] 牛艳娥, 赵芃沛, 李 宁 等. 国内外超高强度钢的研究现状及应用 [J]. 兵器装备工程学报, 2021, 42(7): 274
[36] Zhou C, Ye Q B, Tian Y, et al. Research and application progress of ultra-high strength structural steel [J]. Trans. Mater. Heat Treat., 2021, 42(1): 14
[36] 周 成, 叶其斌, 田 勇 等. 超高强度结构钢的研究及发展 [J]. 材料热处理学报, 2021, 42(1): 14
[37] Yin H, Li J X, Su Y J, et al. Current situation and development of maraging steel [J]. J. Iron Steel Res., 2014, 26(3): 1
[37] 尹 航, 李金许, 宿彦京 等. 马氏体时效钢的研究现状与发展 [J]. 钢铁研究学报, 2014, 26(3): 1
[38] Jiang S H, Wang H, Wu Y, et al. Ultrastrong steel via minimal lattice misfit and high-density nanoprecipitation [J]. Nature, 2017, 544: 460
doi: 10.1038/nature22032
[39] Olson G B. Genomic materials design: The ferrous frontier [J]. Acta Mater., 2013, 61: 771
doi: 10.1016/j.actamat.2012.10.045
[40] Xu W, Rivera-Díaz-del-Castillo P E J, Yan W, et al. A new ultrahigh-strength stainless steel strengthened by various coexisting nanoprecipitates [J]. Acta Mater., 2010, 58: 4067
doi: 10.1016/j.actamat.2010.03.005
[41] Jiao Z B, Luan J H, Miller M K, et al. Precipitation mechanism and mechanical properties of an ultra-high strength steel hardened by nanoscale NiAl and Cu particles [J]. Acta Mater., 2015, 97: 58
doi: 10.1016/j.actamat.2015.06.063
[42] Jiao Z B, Luan J H, Miller M K, et al. Co-precipitation of nanoscale particles in steels with ultra-high strength for a new era [J]. Mater. Today, 2017, 20: 142
doi: 10.1016/j.mattod.2016.07.002
[43] Niu M C, Yin L C, Yang K, et al. Synergistic alloying effects on nanoscale precipitation and mechanical properties of ultrahigh-strength steels strengthened by Ni3Ti, Mo-enriched, and Cr-rich co-precipitates [J]. Acta Mater., 2021, 209: 116788
doi: 10.1016/j.actamat.2021.116788
[44] Wang L J, Jiang S H, Peng B, et al. Ultrastrong steel strengthened by multiple shearable nanostructures [J]. J. Mater. Sci. Technol., 2023, 161: 245
doi: 10.1016/j.jmst.2023.05.001
[45] Raabe D, Ponge D, Dmitrieva O, et al. Nanoprecipitate-hardened 1.5 GPa steels with unexpected high ductility [J]. Scr. Mater., 2009, 60: 1141
doi: 10.1016/j.scriptamat.2009.02.062
[46] Sun L, Simm T H, Martin T L, et al. A novel ultra-high strength maraging steel with balanced ductility and creep resistance achieved by nanoscale β-NiAl and Laves phase precipitates [J]. Acta Mater., 2018, 149: 285
doi: 10.1016/j.actamat.2018.02.044
[47] Sun M X, Zhang W N, Liu Z Y, et al. Direct observations on the crystal structure evolution of nano Cu-precipitates in an extremely low carbon steel [J]. Mater. Lett., 2017, 187: 49
doi: 10.1016/j.matlet.2016.10.077
[48] Bhadeshia H K D H, Edmonds D V. The bainite transformation in a silicon steel [J]. Metall. Trans., 1979, 10A: 895
[49] Hodgson P, Timokhina I, Xiong X Y, et al. Understanding of the bainite transformation in a nano-structured bainitic steel [J]. Solid State Phenom., 2011, 172-174: 123
doi: 10.4028/www.scientific.net/SSP.172-174
[50] He B B, Hu B, Yen H W, et al. High dislocation density-induced large ductility in deformed and partitioned steels [J]. Science, 2017, 357: 1029
doi: 10.1126/science.aan0177 pmid: 28839008
[51] Qin S W, Liu Y, Hao Q G, et al. High carbon microalloyed martensitic steel with ultrahigh strength-ductility [J]. Mater. Sci. Eng., 2016, A663: 151
[52] Gao G H, Zhang H, Gui X L, et al. Enhanced ductility and toughness in an ultrahigh-strength Mn-Si-Cr-C steel: The great potential of ultrafine filmy retained austenite [J]. Acta Mater., 2014, 76: 425
doi: 10.1016/j.actamat.2014.05.055
[53] Yin C C, Hu F, Zheng H, et al. Research progress on retained austenite refinement and controlling of mechanical properties of nanostructured bainitic steel [J]. Trans. Mater. Heat Treat., 2021, 42(1): 1
[53] 尹朝朝, 胡 锋, 郑 花 等. 纳米贝氏体钢残奥细化及其力学性能调控研究进展 [J]. 材料热处理学报, 2021, 42(1): 1
doi: 10.13289/j.issn.1009-6264.2020-0277
[54] Wilms M B, Rittinghaus S K, Goßling M, et al. Additive manufacturing of oxide-dispersion strengthened alloys: Materials, synthesis and manufacturing [J]. Prog. Mater. Sci., 2023, 133: 101049
doi: 10.1016/j.pmatsci.2022.101049
[55] Romero-Resendiz L, El-Tahawy M, Zhang T, et al. Heterostructured stainless steel: Properties, current trends, and future perspectives [J]. Mater. Sci. Eng., 2022, R150: 100691
[56] Nagarajan B, Hu Z H, Song X, et al. Development of micro selective laser melting: The state of the art and future perspectives [J]. Engineering, 2019, 5: 702
doi: 10.1016/j.eng.2019.07.002
[57] Yadroitsev I, Smurov I. Selective laser melting technology: From the single laser melted track stability to 3D parts of complex shape [J]. Phys. Proc., 2010, 5: 551
doi: 10.1016/j.phpro.2010.08.083
[58] Thompson S M, Bian L K, Shamsaei N, et al. An overview of Direct Laser Deposition for additive manufacturing; Part I: Transport phenomena, modeling and diagnostics [J]. Addit. Manuf., 2015, 8: 36
[59] Ding D H, Pan Z X, Cuiuri D, et al. Wire-feed additive manufacturing of metal components: Technologies, developments and future interests [J]. Int. J. Adv. Manuf. Technol., 2015, 81: 465
doi: 10.1007/s00170-015-7077-3
[60] Wu W W, Xiang C, Zhang T, et al. Effect of heat treatment on microstructure and mechanical properties of 18Ni300 maraging steel fabricated by selective laser melting [J]. Acta Metall. Sin., 2025, 61: 1515
doi: 10.11900/0412.1961.2024.00009
[60] 吴文伟, 向 超, 张 涛 等. 热处理工艺对选区激光熔化成型18Ni300马氏体时效钢微观组织及力学性能的影响 [J]. 金属学报, 2025, 61: 1515
doi: 10.11900/0412.1961.2024.00009
[61] Tan C L, Zhou K S, Ma W Y, et al. Microstructural evolution, nanoprecipitation behavior and mechanical properties of selective laser melted high-performance grade 300 maraging steel [J]. Mater. Des., 2017, 134: 23
doi: 10.1016/j.matdes.2017.08.026
[62] Tan C L, Zhou K S, Kuang M, et al. Microstructural characterization and properties of selective laser melted maraging steel with different build directions [J]. Sci. Technol. Adv. Mater., 2018, 19: 746
doi: 10.1080/14686996.2018.1527645
[63] Jägle E A, Choi P P, Van Humbeeck J, et al. Precipitation and austenite reversion behavior of a maraging steel produced by selective laser melting [J]. J. Mater. Res., 2014, 29: 2072
doi: 10.1557/jmr.2014.204
[64] Becker T H, Dimitrov D. The achievable mechanical properties of SLM produced maraging Steel 300 components [J]. Rapid Prototyping J., 2016, 22: 487
doi: 10.1108/RPJ-08-2014-0096
[65] Suryawanshi J, Prashanth K G, Ramamurty U. Tensile, fracture, and fatigue crack growth properties of a 3D printed maraging steel through selective laser melting [J]. J. Alloys Compd., 2017, 725: 355
doi: 10.1016/j.jallcom.2017.07.177
[66] Tan C L, Zhou K S, Ma W Y, et al. Interfacial characteristic and mechanical performance of maraging steel-copper functional bimetal produced by selective laser melting based hybrid manufacture [J]. Mater. Des., 2018, 155: 77
doi: 10.1016/j.matdes.2018.05.064
[67] Cyr E, Asgari H, Shamsdini S, et al. Fracture behaviour of additively manufactured MS1-H13 hybrid hard steels [J]. Mater. Lett., 2018, 212: 174
doi: 10.1016/j.matlet.2017.10.097
[68] Wang B X, Cui W W, Zhang Y, et al. Effect of tempering temperature on microstructure and mechanical properties of 300M steel [J]. Foundry Technol., 2021, 42: 719
[68] 王丙旭, 崔威威, 张 宇 等. 回火温度对300M钢组织和性能的影响 [J]. 铸造技术, 2021, 42: 719
[69] Wen C F, Xiao A D, Liu X H, et al. Effect of tempering temperature on microstructure and mechanical properties of low alloy ultra-high strength steel Q1300 [J]. Heat Treat. Met., 2019, 44(2): 172
[69] 温长飞, 肖爱达, 刘旭辉 等. 回火温度对低合金超高强钢Q1300组织与性能的影响 [J]. 金属热处理, 2019, 44(2): 172
[70] Abdollah-Zadeh A, Jafari-Pirlari A, Barzegari M. Tempered martensite embrittlement in a 32NiCrMoV125 steel [J]. J. Mater. Eng. Perform., 2005, 14: 569
doi: 10.1361/105994905X64657
[71] Kim S H, Kim H, Kim N J. Brittle intermetallic compound makes ultrastrong low-density steel with large ductility [J]. Nature, 2015, 518: 77
doi: 10.1038/nature14144
[72] Li X Y, Lu K. Improving sustainability with simpler alloys [J]. Science, 2019, 364: 733
doi: 10.1126/science.aaw9905 pmid: 31123122
[73] Jan-Erik A, Lindberg F, Patrik Ö. Hybrid steel enhances component performance at reduced weight [J]. Lightweight Des. Worldw., 2019, 12: 34
[74] Ma X L, Zhang C C, Zhang C L, et al. Microstructure and properties of sorbite stainless steel designed by “hybrid” idea [J]. Mater. Rep., 2020, 34: 4103
[74] 马潇磊, 张成成, 张朝磊 等. 基于“混杂”设计的索氏体新型不锈钢的组织和性能 [J]. 材料导报, 2020, 34: 4103
[75] Pan X K, Huang B Y, Zhang C L, et al. Strengthening mechanism and precipitate evolution of a multi-application special engineering steel designed based on a hybrid idea [J]. J. Alloys Compd., 2023, 942: 169053
doi: 10.1016/j.jallcom.2023.169053
[76] Lee J Y, Jeong H B, Jo W H, et al. Hydrogen desorption mechanism associated with ε carbide decomposition in martensitic medium-Mn steel [J]. J. Mater. Res. Technol., 2025, 37: 3832
doi: 10.1016/j.jmrt.2025.07.082
[77] Chen J Y, Jin P F, Wang S J, et al. A novel Ni-Mo-W-V martensitic steel for hot working dies: Improved elevated-temperature mechanical properties and wear resistance via thermally stable MC nanoprecipitates [J]. Tribol. Int., 2025, 207: 110618
doi: 10.1016/j.triboint.2025.110618
[78] Hong C W, Youn K T, Kim S H, et al. Investigation of V-rich MC (M = V, Mo) carbide behavior related to thermal fatigue property in commercial hot work tool steel processing [J]. Mater. Charact., 2024, 214: 114025
doi: 10.1016/j.matchar.2024.114025
[79] Ghosh G, Olson G B. Precipitation of paraequilibrium cementite: Experiments, and thermodynamic and kinetic modeling [J]. Acta Mater., 2002, 50: 2099
doi: 10.1016/S1359-6454(02)00054-X
[80] Dyson D J, Keown S R, Raynor D, et al. The orientation relationship and growth direction of Mo2C in ferrite [J]. Acta Metall., 1966, 14: 867
doi: 10.1016/0001-6160(66)90007-1
[81] Wang C C. Alloy design of high Co-Ni secondary hardening steel by multi-scale simulation [D]. Beijing: Tsinghua University, 2017
[81] 王晨充. 基于多尺度模拟的高Co-Ni二次硬化钢合金设计 [D]. 北京: 清华大学, 2017
[82] Kamikawa N, Abe Y, Miyamoto G, et al. Tensile behavior of Ti, Mo-added low carbon steels with interphase precipitation [J]. ISIJ Int., 2014, 54: 212
doi: 10.2355/isijinternational.54.212
[83] Jain D, Isheim D, Hunter A H, et al. Multicomponent high-strength low-alloy steel precipitation-strengthened by sub-nanometric Cu precipitates and M2C carbides [J]. Metall. Mater. Trans., 2016, 47A: 3860
[84] Inoue A, Masumoto T. Carbide reactions (M3C→M7C3→M23C6→M6C) during tempering of rapidly solidified high carbon Cr-W and Cr-Mo steels [J]. Metall. Trans., 1980, 11A: 739
[85] Kapoor M, Isheim D, Ghosh G, et al. Aging characteristics and mechanical properties of 1600MPa body-centered cubic Cu and B2-NiAl precipitation-strengthened ferritic steel [J]. Acta Mater., 2014, 73: 56
doi: 10.1016/j.actamat.2014.03.051
[86] Li C N, Duan R, Fu W, et al. Improvement of mechanical properties for low carbon ultra-high strength steel strengthened by Cu-rich multistructured precipitation via modification to bainite [J]. Mater. Sci. Eng., 2021, A817: 141337
[87] Moshka O, Pinkas M, Brosh E, et al. Addressing the issue of precipitates in maraging steels—Unambiguous answer [J]. Mater. Sci. Eng., 2015, A638: 232
[88] Simm T H, Sun L, Galvin D R, et al. A SANS and APT study of precipitate evolution and strengthening in a maraging steel [J]. Mater. Sci. Eng., 2017, A702: 414
[89] Ruan T T, Shen J J, Li B, et al. High-temperature strengthening mechanism and thermal stability of Laves phase in ferritic matrix [J]. Mater. Sci. Eng., 2022, A859: 144183
[90] Zhang C X, Gao Q Z, Ma Q S, et al. Variety of yield strength caused by precipitations of L12-Ni3Al and B2-NiAl phases in alumina-forming austenitic steel [J]. Mater. Sci. Eng., 2024, A894: 146177
[91] Jiao Z B, Luan J H, Miller M K, et al. Group precipitation and age hardening of nanostructured Fe-based alloys with ultra-high strengths [J]. Sci. Rep., 2016, 6: 21364
doi: 10.1038/srep21364 pmid: 26892834
[92] Leitner H, Schober M, Schnitzer R. Splitting phenomenon in the precipitation evolution in an Fe-Ni-Al-Ti-Cr stainless steel [J]. Acta Mater., 2010, 58: 1261
doi: 10.1016/j.actamat.2009.10.030
[93] Schnitzer R, Schober M, Zinner S, et al. Effect of Cu on the evolution of precipitation in an Fe-Cr-Ni-Al-Ti maraging steel [J]. Acta Mater., 2010, 58: 3733
doi: 10.1016/j.actamat.2010.03.010
[94] Liebscher C H, Radmilović V R, Dahmen U, et al. A hierarchical microstructure due to chemical ordering in the bcc lattice: Early stages of formation in a ferritic Fe-Al-Cr-Ni-Ti alloy [J]. Acta Mater., 2015, 92: 220
doi: 10.1016/j.actamat.2015.03.043
[95] Millán J, Sandlöbes S, Al-Zubi A, et al. Designing Heusler nanoprecipitates by elastic misfit stabilization in Fe-Mn maraging steels [J]. Acta Mater., 2014, 76: 94
doi: 10.1016/j.actamat.2014.05.016
[96] Delagnes D, Pettinari-Sturmel F, Mathon M H, et al. Cementite-free martensitic steels: A new route to develop high strength/high toughness grades by modifying the conventional precipitation sequence during tempering [J]. Acta Mater., 2012, 60: 5877
doi: 10.1016/j.actamat.2012.07.030
[97] Wang Y X, Guo X F, Hu C D, et al. Industrially produced 2.4 GPa ultra-strong steel via nanoscale dual-precipitates co-configuration [J]. Mater. Charact., 2024, 208: 113646
doi: 10.1016/j.matchar.2024.113646
[98] Wang Y X, Li A J, Wang T, et al. Effects of NiAl on precipitation behavior and mechanical properties of M2C strengthened secondary hardening steel [J]. J. Mater. Res. Technol., 2025, 35: 3107
doi: 10.1016/j.jmrt.2025.02.002
[99] Zhu H F, Xiong Z P, Mao J W, et al. Effect of ageing temperature on the microstructural evolution and mechanical properties in M2C and NiAl co-precipitation secondary hardening ultrahigh-strength steel [J]. J. Mater. Res. Technol., 2024, 30: 3522
doi: 10.1016/j.jmrt.2024.04.116
[100] Liu X Q, Wang C C, Zhang Y F, et al. Design of a 2.7 GPa ultra-high-strength high Co-Ni secondary hardening steel by two-step nano-size precipitation tailoring [J]. J. Mater. Res. Technol., 2024, 28: 4212
doi: 10.1016/j.jmrt.2024.01.038
[101] Xiao C J, Zhang Y P, Zhan D P, et al. Effect of Cu addition on the precipitation behavior of M2C carbides in maraging steel [J]. Mater. Charact., 2024, 210: 113846
doi: 10.1016/j.matchar.2024.113846
[102] Peng R Z, Wu X C, Chen S N, et al. Evolution mechanism of Mo-rich, B2-NiAl, and Cu-rich particles under aging and its influence on strength and elongation in a maraging hot work steel SDH88 [J]. Mater. Sci. Eng., 2024, A916: 147317
[103] Galindo-Nava E I, Rainforth W M, Rivera-Díaz-del-Castillo P E J. Predicting microstructure and strength of maraging steels: Elemental optimisation [J]. Acta Mater., 2016, 117: 270
doi: 10.1016/j.actamat.2016.07.020
[104] Galindo-Nava E I, Rivera-Díaz-del-Castillo P E J. A model for the microstructure behaviour and strength evolution in lath martensite [J]. Acta Mater., 2015, 98: 81
doi: 10.1016/j.actamat.2015.07.018
[105] Follansbee P S, Kocks U F. A constitutive description of the deformation of copper based on the use of the mechanical threshold stress as an internal state variable [J]. Acta Metall., 1988, 36: 81
doi: 10.1016/0001-6160(88)90030-2
[106] Fleischer R L. Substitutional solution hardening [J]. Acta Metall., 1963, 11: 203
doi: 10.1016/0001-6160(63)90213-X
[107] Labusch R. A statistical theory of solid solution hardening [J]. Phys. Satus Solidi, 1970, 41b: 659
[108] Li Y J, Yuan G, Li L L, et al. Ductile 2-GPa steels with hierarchical substructure [J]. Science, 2023, 379: 168
doi: 10.1126/science.add7857 pmid: 36634172
[109] Kimura Y, Inoue T, Yin F X, et al. Inverse temperature dependence of toughness in an ultrafine grain-structure steel [J]. Science, 2008, 320: 1057
doi: 10.1126/science.1156084 pmid: 18497294
[110] Li Y Z, Huang M X. A method to calculate the dislocation density of a TWIP steel based on neutron diffraction and synchrotron X-ray diffraction [J]. Acta Metall. Sin., 2020, 56: 487
doi: 10.11900/0412.1961.2020.00016
[110] 李亦庄, 黄明欣. 基于中子衍射和同步辐射X射线衍射的TWIP钢位错密度计算方法 [J]. 金属学报, 2020, 56: 487
doi: 10.11900/0412.1961.2020.00016
[111] Cong Z H, Murata Y. Dislocation density of lath martensite in 10Cr-5W heat-resistant steels [J]. Mater. Trans., 2011, 52: 2151
doi: 10.2320/matertrans.M2011201
[112] Blankenship C P, Hornbogen E, Starke E A. Predicting slip behavior in alloys containing shearable and strong particles [J]. Mater. Sci. Eng., 1993, A169: 33
[113] Yong Q L. Secondary Phases in Steel [M]. Beijing: Metallurgical Industry Press, 2006: 442
[113] 雍岐龙. 钢铁材料中的第二相 [M]. 北京: 冶金工业出版社, 2006: 442
[114] Ma K K, Wen H M, Hu T, et al. Mechanical behavior and strengthening mechanisms in ultrafine grain precipitation-strengthened aluminum alloy [J]. Acta Mater., 2014, 62: 141
doi: 10.1016/j.actamat.2013.09.042
[115] Götz G, Blum W. Influence of thermal history on precipitation of hardening phases in tempered martensite 10%Cr-steel X12CrMo-WVNbN 10-1-1 [J]. Mater. Sci. Eng., 2003, A348: 201
[116] Wang F, Song M, Elkot M N, et al. Shearing brittle intermetallics enhances cryogenic strength and ductility of steels [J]. Science, 2024, 384: 1017
doi: 10.1126/science.ado2919 pmid: 38815014
[117] Kapoor M. Design and development of bcc-copper- and B2 nickel-aluminium-precipitation-strengthened ferritic steel [D]. Evanston: Northwestern University, 2013
[118] Aghajani A, Somsen C, Eggeler G. On the effect of long-term creep on the microstructure of a 12% chromium tempered martensite ferritic steel [J]. Acta Mater., 2009, 57: 5093
doi: 10.1016/j.actamat.2009.07.010
[119] Zhang T Y, Zhang B, Xiao N, et al. Effect of austenitizing temperature on the microstructure and mechanical properties of a 2 GPa ultra-high strength steel [J]. Acta Metall. Sin., 2025, 61: 1353
doi: 10.11900/0412.1961.2024.00005
[119] 张天宇, 张 鹏, 肖 娜 等. 奥氏体化温度对2 GPa超高强钢显微组织和力学性能的影响 [J]. 金属学报, 2025, 61: 1353
doi: 10.11900/0412.1961.2024.00005
[120] Baird J D. The effects of strain-ageing due to interstitial solutes on the mechanical properties of metals [J]. Metall. Rev., 1971, 16: 1
[121] Zener C. Theory of growth of spherical precipitates from solid solution [J]. J. Appl. Phys., 1949, 20: 950
doi: 10.1063/1.1698258
[122] Gladman T. On the theory of the effect of precipitate particles on grain growth in metals [J]. Proc. Roy. Soc., 1966, 294A: 298
[123] Baldan A. Review Progress in Ostwald ripening theories and their applications to nickel-base superalloys Part I: Ostwald ripening theories [J]. J. Mater. Sci., 2002, 37: 2171
doi: 10.1023/A:1015388912729
[124] Lifshitz I M, Slyozov V V. The Kinetics of precipitation from supersaturated solid solutions [J]. J. Phys. Chem. Solids, 1961, 19: 35
doi: 10.1016/0022-3697(61)90054-3
[125] Wagner C. Theorie der alterung von niederschlägen durch umlösen (Ostwald-Reifung) [J]. Z. Electrochemie, Ber. Bunsen. Phys. Chem., 1961, 65: 581
[126] Speight M V. Growth kinetics of grain-boundary precipitates [J]. Acta Metall., 1968, 16: 133
doi: 10.1016/0001-6160(68)90081-3
[127] Kirchner H O K. Coarsening of grain-boundary precipitates [J]. Metall. Trans., 1971, 2: 2861
[128] Ardell A J. On the coarsening of grain boundary precipitates [J]. Acta Metall., 1972, 20: 601
doi: 10.1016/0001-6160(72)90015-6
[1] 欧阳求保, 苏楠, 王瑞安, 刘侃, 张荻. 跨尺度协同增强铝基复合材料研究进展[J]. 金属学报, 2026, 62(5): 733-742.
[2] 江慧敏, 魏梦洁, 胡小强, 蔡欣, 李殿中, 党恩. 回火温度对超深井承压件F22M钢微观组织与力学性能的影响[J]. 金属学报, 2026, 62(4): 587-598.
[3] 曹艳飞, 张潇, 刘宏伟, 王磊涛, 柯于斌, 何伦华, 谢振华, 王培, 李殿中. 深冷处理M50航发轴承钢中纳米碳化物析出与残余应力演化的中子研究[J]. 金属学报, 2026, 62(3): 467-476.
[4] 郑沁园, 刘朋, 路轶, 朱海龙, 郑成武, 栾义坤, 李殿中. 预先Mn配分对中锰钢中温连续冷却过程中贝氏体相变的影响[J]. 金属学报, 2026, 62(3): 477-488.
[5] 赵霞, 王旻, 郝宪朝, 张龙, 高明, 马颖澈, 刘奎. 晶界碳化物和动态再结晶对690合金柱状晶凝固组织高温塑性的影响[J]. 金属学报, 2026, 62(2): 339-350.
[6] 张天昊, 鞠泉, 蒙肇斌, 王浩, 胡本芙. GH3230合金薄板填丝钨极氩弧焊接头的组织稳定性[J]. 金属学报, 2025, 61(9): 1375-1386.
[7] 刘继浩, 迟宏宵, 武会宾, 马党参, 周健, 谷金波. 喷射成形工艺对M3高速钢碳化物特征及力学性能的影响[J]. 金属学报, 2025, 61(8): 1229-1244.
[8] 谢昂, 陈胜虎, 姜海昌, 戎利建. Nb含量和均质化处理对奥氏体不锈钢铸态组织和力学性能的影响[J]. 金属学报, 2025, 61(7): 1035-1048.
[9] 李夫顺, 刘志鹏, 丁灿灿, 胡斌, 罗海文. 一种新型高强奥氏体低密度钢的强塑性机理[J]. 金属学报, 2025, 61(6): 909-916.
[10] 赵广迪, 李阳, 姚晓雨, 王亮, 李渭滨, 潘玉华, 李维娟, 王兆宇. B对Fe-Cr-B-C合金凝固行为、强韧性及耐磨性的影响[J]. 金属学报, 2025, 61(5): 699-716.
[11] 梁炫, 侯廷平, 张东, 谭昕暘, 吴开明. 中碳Nb合金化钢液析碳化物的析出行为[J]. 金属学报, 2025, 61(4): 653-664.
[12] 韩启飞, 狄兴隆, 郭跃岭, 叶水俊, 郑元翾, 刘长猛. 电弧熔丝增材制造Mg/Mg双金属的组织与力学性能[J]. 金属学报, 2025, 61(2): 211-225.
[13] 鞠玉琳, 魏琪, 袁志钟, 程晓农. 低合金高强钢板贝/马复相回火过程硬度及微观组织的演变行为[J]. 金属学报, 2025, 61(10): 1531-1541.
[14] 马芳, 陆星宇, 周丽娜, 杜宁宇, 类承帅, 刘宏伟, 李殿中. M50钢中 M2C一次碳化物高温转变机制[J]. 金属学报, 2024, 60(7): 901-914.
[15] 徐洋, 柯黎明, 聂浩, 夏春, 刘强, 陈书锦. 局部强冷作用下厚板铝合金/镁合金搅拌摩擦焊界面金属间化合物的析出行为[J]. 金属学报, 2024, 60(6): 777-788.