Please wait a minute...
金属学报  2026, Vol. 62 Issue (7): 1175-1188    DOI: 10.11900/0412.1961.2025.00203
  综述 本期目录 | 过刊浏览 |
Nb稳定化奥氏体不锈钢在第四代核电领域的研究进展
陈胜虎1,2(), 谢昂1, 杨彬彬2, 刘涌涛2, 陈思含1, 赵明久1,2, 姜海昌1,2, 戎利建1,2()
1 中国科学院金属研究所 中国科学院核用材料与安全评价重点实验室 沈阳 110016
2 中国科学技术大学 材料科学与工程学院 沈阳 110016
Research Progress of the Niobium-Stabilized Austenitic Stainless Steels for Generation-IV Nuclear Reactors
CHEN Shenghu1,2(), XIE Ang1, YANG Binbin2, LIU Yongtao2, CHEN Sihan1, ZHAO Mingjiu1,2, JIANG Haichang1,2, RONG Lijian1,2()
1 CAS Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
2 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
引用本文:

陈胜虎, 谢昂, 杨彬彬, 刘涌涛, 陈思含, 赵明久, 姜海昌, 戎利建. Nb稳定化奥氏体不锈钢在第四代核电领域的研究进展[J]. 金属学报, 2026, 62(7): 1175-1188.
Shenghu CHEN, Ang XIE, Binbin YANG, Yongtao LIU, Sihan CHEN, Mingjiu ZHAO, Haichang JIANG, Lijian RONG. Research Progress of the Niobium-Stabilized Austenitic Stainless Steels for Generation-IV Nuclear Reactors[J]. Acta Metall Sin, 2026, 62(7): 1175-1188.

全文: PDF(2518 KB)   HTML
摘要: 

奥氏体不锈钢因其良好的综合性能、成熟的制造工艺以及在压水反应堆中数十年的服役经验,是第四代核电反应堆核心部件的候选材料。然而,在长期高温、强辐照环境下,奥氏体不锈钢暴露出蠕变强度不足、组织稳定性较差、辐照脆化敏感性较高等不足。近年来,Nb元素的合金化可有效调控奥氏体不锈钢的第二相析出行为及辐照缺陷的形成和演化过程,有望实现高温蠕变性能与抗辐照性能的同步提升,成为开发新一代耐高温、抗辐照、长寿命奥氏体不锈钢的重要途径。本文系统综述了Nb稳定化奥氏体不锈钢在四代核电领域的研究进展,重点从高温蠕变性能和抗辐照性能提升的角度,回顾了其成分设计与优化的发展历程及应用现状,分析了Nb添加对奥氏体稳定性、初生NbC形成机制以及含Nb第二相析出和强化机制的影响,探讨了其对强韧性、蠕变强度、高温组织稳定性、辐照诱发缺陷演化的调节机制,并对未来Nb稳定化奥氏体不锈钢的发展进行了展望。

关键词 : Nb稳定化奥氏体不锈钢,  强韧性匹配,  蠕变强度,  高温组织稳定性,  辐照诱发缺陷,  含Nb第二相    
Abstract:

Austenitic stainless steels are utilized in the in-core and out-of-core structural components of various Generation-IV nuclear reactors owing to their excellent comprehensive properties, mature manufacturing processes, and decades of service experience in pressurized water reactors. However, after prolonged exposure to high temperature and high-intensity irradiation, these steels gradually exhibit some performance limitations, including lower creep strength, inadequate microstructural stabilities, and higher radiation embrittlement sensitivities. Recently, alloying with Nb has been proven to effectively regulate the precipitation behavior of secondary phases and the formation and evolution of irradiation defects in austenitic stainless steels, promising simultaneous improvements in creep strength and irradiation tolerance. Therefore, Nb alloying has emerged as a key pathway for the development of next-generation austenitic stainless steels with enhanced high-temperature performance, improved irradiation resistance, and extended service life. This paper systematically reviews the research progress of Nb-stabilized austenitic stainless steels for Generation-IV nuclear power applications, including the compositional design and optimization to improve the creep properties and irradiation resistance, the effects of Nb addition on austenite stability, the formation mechanisms of primary NbC, and the precipitation behavior of Nb-bearing secondary phases. Additionally, the mechanisms by which Nb alloying influences the strength-ductility balance, creep strength, high-temperature microstructural stability, and irradiation-induced defect evolution are discussed. Finally, some future research prospects of Nb-stabilized austenitic stainless steels for Generation-IV nuclear reactors are discussed.

Key words: niobium-stabilized austenitic stainless steel    strength-ductility balance    creep strength    high-temperature microstructural stability    irradiation-induced defect    Nb-bearing secondary phase
收稿日期: 2025-07-15     
ZTFLH:  TG142.25  
基金资助:中国科学院战略性先导科技专项(XDA0410000);中核集团领创科研项目
通讯作者: 陈胜虎,chensh@imr.ac.cn,主要从事核用结构材料研究;
戎利建,ljrong@imr.ac.cn,主要从事特种合金研究
Corresponding author: CHEN Shenghu, professor, Tel: (024)23971981, E-mail: chensh@imr.ac.cn;
作者简介: 陈胜虎,男,1986年生,研究员,博士
Reactor systemCoolantOutlet temperature / oCNeutron spectrum, maximum dose

Sodium fast reactor

Lead fast reactor

Gas fast reactor

Supercritical water reactor

Very high temperature reactor

Molten salt reactor

Sodium

Lead or lead-bismuth

Helium

Supercritical water

Helium

Molten salt

500-550

480-570

~850

510-625

900-1000

700-800

Fast, 150 dpa

Fast, 100 dpa

Fast, 90 dpa

Fast/thermal, 70 dpa

Thermal, 20 dpa

Thermal, 200 dpa

表1  六种第四代反应堆系统的服役工况[6~10]
TypeCNiCrMnMoSiNbTiVN

EP302

347H

TP347HFG

316Nb

FV548

DIN1.4981

EI847

PNC316

PNC1520

EK164

Alloy 709

HT-UPS

0.08-0.12

0.04-0.10

0.06-0.10

≤ 0.08

0.1

0.04-0.10

0.04-0.06

0.06

0.06

0.05-0.09

≤ 0.10

0.08

8.0-10.0

9.0-13.0

9.0-13.0

10.0-14.0

11.5

15.5-17.5

15.0-16.0

14.0

20.0

18.0-19.5

23.0-26.0

16.0

14.0-16.0

17.0-19.0

17.0-19.0

16.0-18.0

16.5

15.5-17.5

15.0-16.0

16.0

15.0

15.0-16.5

19.5-23.0

14.0

0.4-0.8

≤ 2.0

≤ 2.0

≤ 2.0

1.2

≤ 1.5

0.4-0.8

1.7

1.7

1.5-2.0

≤ 1.5

2.0

-

-

-

2.0-3.0

1.5

1.6-2.0

2.7-3.2

2.5

2.5

2.0-2.5

1.0-2.0

2.5

2.2-3.0

≤ 0.75

≤ 1.0

≤ 0.75

0.35

0.3-0.6

≤ 0.4

0.6

0.5

0.3-0.6

≤ 1.0

0.4

0.7-1.0

8C-1.0

8C-1.0

10C-1.0

0.7

10C-1.2

≤ 0.9

(Nb + Ta): 0.08

0.1

0.1-0.4

0.1-0.4

0.1

-

-

-

-

-

-

-

0.1

0.25

0.25-0.5

0.02-0.2

0.3

-

-

-

-

-

-

-

-

-

0.15

-

0.5

-

-

-

≤ 0.1

-

-

-

-

-

-

0.1-0.25

-

表2  先进核电反应堆用含Nb奥氏体不锈钢的化学成分[44~46] (mass fraction / %)
图1  不同Nb含量Fe-15Cr-10Ni氏体不锈钢的铸态组织
图2  Nb含量对Fe-15Cr-10Ni奥氏体不锈钢中NbC析出行为的热力学模拟计算与含0.9%Nb铸态组织的OM像
图3  铸态试样中初生NbC和奥氏体的纳米压痕结果及室温变形后组织形貌的TEM像[62]
图4  Fe-15Cr-10Ni奥氏体不锈钢中初生NbC的三维分布形貌及室温冲击断裂后组织形貌的SEM像和Nb元素EDS面扫描图
图5  不同牌号奥氏体不锈钢的高温蠕变强度
图6  Alloy 709和HT-UPS奥氏体不锈钢经高温服役后的第二相形貌[76,77]及MC碳化物EDS分析
图7  316L钢和Nb稳定化20Cr25Ni奥氏体不锈钢的温度-时间-析出(TTP)曲线[80,81]
图8  Nb稳定化奥氏体不锈钢中G相和σ相形成机理示意图
图9  Nb添加对Fe-16Ni-15Cr合金50 dpa离子辐照条件下空洞密度和直径的影响[92]
图10  NbC/基体界面捕获点缺陷的微观机制[96]
图11  Nb稳定化奥氏体不锈钢的综合性能评估[104]
[1] Buckthorpe D. Introduction to Generation IV nuclear reactors [A]. Structural Materials for Generation IV Nuclear Reactors [M]. Amsterdam: Woodhead Publishing, 2017: 1
[2] Kelly J E. Generation IV International Forum: A decade of progress through international cooperation [J]. Prog. Nucl. Energy, 2014, 77: 240
doi: 10.1016/j.pnucene.2014.02.010
[3] Locatelli G, Mancini M, Todeschini N. Generation IV nuclear reactors: Current status and future prospects [J]. Energy Policy, 2013, 61: 1503
doi: 10.1016/j.enpol.2013.06.101
[4] Pioro I L, Rodriguez G H. Generation IV international forum (GIF) [A]. Handbook of Generation IV Nuclear Reactors [M]. Cambridge: Woodhead Publishing, 2023: 111
[5] China Nuclear Energy Association, Hualong Nuclear Power Technology Co., Ltd. Blue Book of China Nuclear Energy Development Report [M]. Beijing: Scientific and Technical Documentaton Press, 2025: 1
[5] 中国核能行业协会, 华龙国际核电技术有限公司. 中国核能科技创新发展报告 [M]. 北京: 科学技术文献出版社, 2025: 1
[6] Abram T, Ion S. Generation-IV nuclear power: A review of the state of the science [J]. Energy Policy, 2008, 36: 4323
doi: 10.1016/j.enpol.2008.09.059
[7] Lorusso P, Bassini S, Del Nevo A, et al. GEN-IV LFR development: Status perspectives [J]. Prog. Nucl. Energy, 2018, 105: 318
doi: 10.1016/j.pnucene.2018.02.005
[8] Magwood IV W D, Paillere H. Looking ahead at reactor development [J]. Prog. Nucl. Energy, 2018, 102: 58
doi: 10.1016/j.pnucene.2017.07.001
[9] Serp J, Allibert M, Beneš O, et al. The molten salt reactor (MSR) in generation IV: Overview and perspectives [J]. Prog. Nucl. Energy, 2014, 77: 308
doi: 10.1016/j.pnucene.2014.02.014
[10] Guérin Y, Was G S, Zinkle S J. Materials challenges for advanced nuclear energy systems [J]. MRS Bull., 2009, 34: 10
[11] Yvon P, Carré F. Structural materials challenges for advanced reactor systems [J]. J. Nucl. Mater., 2009, 385: 217
doi: 10.1016/j.jnucmat.2008.11.026
[12] Murty K L, Charit I. Structural materials for Gen-IV nuclear reactors: Challenges and opportunities [J]. J. Nucl. Mater., 2008, 383: 189
doi: 10.1016/j.jnucmat.2008.08.044
[13] Gong X, Short M P, Auger T, et al. Environmental degradation of structural materials in liquid lead- and lead-bismuth eutectic-cooled reactors [J]. Prog. Mater. Sci., 2022, 126: 100920
doi: 10.1016/j.pmatsci.2022.100920
[14] Yvon P, Le Flem M, Cabet C, et al. Structural materials for next generation nuclear systems: Challenges and the path forward [J]. Nucl. Eng. Des., 2015, 294: 161
doi: 10.1016/j.nucengdes.2015.09.015
[15] Mansur L K, Rowcliffe A F, Nanstad R K, et al. Materials needs for fusion, Generation IV fission reactors and spallation neutron sources—Similarities and differences [J]. J. Nucl. Mater., 2004, 329-333: 166
doi: 10.1016/j.jnucmat.2004.04.016
[16] Samaras M, Hoffelner W, Victoria M. Modelling of advanced structural materials for GEN IV reactors [J]. J. Nucl. Mater., 2007, 371: 28
doi: 10.1016/j.jnucmat.2007.05.026
[17] Maloy S A, Natesan K, Holcomb D E, et al. Overview of reactor systems and operational environments for structural materials in gen-IV fission reactors [A]. Structural Alloys for Nuclear Energy Applications [M]. Amsterdam: Elsevier, 2019: 23
[18] Was G S, Ukai S. Austenitic stainless steels [A]. Structural Alloys for Nuclear Energy Applications [M]. Amsterdam: Elsevier, 2019: 293
[19] Cheon J S, Lee C B, Lee B O, et al. Sodium fast reactor evaluation: Core materials [J]. J. Nucl. Mater., 2009, 392: 324
doi: 10.1016/j.jnucmat.2009.03.021
[20] Klueh R L. Elevated temperature ferritic and martensitic steels and their application to future nuclear reactors [J]. Int. Mater. Rev., 2005, 50: 287
doi: 10.1179/174328005X41140
[21] Chen S H, Rong L J. Oxide scale formation on ultrafine-grained ferritic-martensitic steel during pre-oxidation and its effect on the corrosion performance in stagnant liquid Pb-Bi eutectic [J]. Acta Metall. Sin., 2021, 57: 989
[21] 陈胜虎, 戎利建. 超细晶铁素体-马氏体钢的高温氧化成膜特性及其对Pb-Bi腐蚀行为的影响 [J]. 金属学报, 2021, 57: 989
doi: 10.11900/0412.1961.2020.00451
[22] Zhao Y Y, Ding S A, Du Y Y, et al. Effect of long-term thermal aging on lead-bismuth eutectic corrosion behavior of 9Cr ferritic/martensitic steel [J]. J. Mater. Sci. Technol., 2025, 210: 299
doi: 10.1016/j.jmst.2024.05.049
[23] Liu S J, Huang Q Y, Peng L, et al. Microstructure and its influence on mechanical properties of CLAM steel [J]. Fusion Eng. Des., 2012, 87: 1628
doi: 10.1016/j.fusengdes.2012.06.008
[24] Ma Z W, Zhou T, Jin P, et al. Influence of temperature on the microstructural evolution of SIMP and T91 steels in liquid lead-bismuth eutectic: Experiments and molecular dynamics simulations [J]. Corros. Sci., 2023, 222: 111411
doi: 10.1016/j.corsci.2023.111411
[25] Yang K, Yan W, Wang Z G, et al. Development of a novel structural material (SIMP steel) for nuclear equipment with balanced resistances to high temperature, radiation and liquid metal corrosion [J]. Acta Metall. Sin., 2016, 52: 1207
[25] 杨 柯, 严 伟, 王志光 等. 核用新型耐高温、抗辐照、耐液态金属腐蚀结构材料——SIMP钢的研究进展 [J]. 金属学报, 2016, 52: 1207
[26] Chen S H, Xie A, Lv X L, et al. Tailoring microstructure of austenitic stainless steel with improved performance for generation-IV fast reactor application: A review [J]. Crystals, 2023, 13: 268
doi: 10.3390/cryst13020268
[27] Wu X Q, Rong L J, Tan J B, et al. Research advance on liquid lead-bismuth eutectic corrosion resistant Si enhanced ferritic/martensitic and austenitic stainless steels [J]. Acta Metall. Sin., 2023, 59: 502
doi: 10.11900/0412.1961.2022.00531
[27] 吴欣强, 戎利建, 谭季波 等. 耐Pb-Bi腐蚀Si增强型铁素体/马氏体钢和奥氏体不锈钢的研究进展 [J]. 金属学报, 2023, 59: 502
doi: 10.11900/0412.1961.2022.00531
[28] Jayakumar T, Mathew M D, Laha K, et al. Materials development for fast reactor applications [J]. Nucl. Eng. Des., 2013, 265: 1175
doi: 10.1016/j.nucengdes.2013.05.001
[29] Maziasz P J, Busby J T. Properties of austenitic steels for nuclear reactor applications [J]. Compr. Nucl. Mater. (Second Ed.), 2020, 7: 303
[30] Maziasz P J. Overview of microstructural evolution in neutron-irradiated austenitic stainless steels [J]. J. Nucl. Mater., 1993, 205: 118
doi: 10.1016/0022-3115(93)90077-C
[31] Chen L L, Luo R, Gao P, et al. Dynamic recrystallization behavior and coincidence site lattice evolution in thermal deformation of 316H stainless steel used in nuclear systems [J]. J. Iron Steel Res. Int., 2023, 30: 1862
doi: 10.1007/s42243-022-00863-8
[32] Mathew M D. Evolution of creep resistant 316 stainless steel for sodium cooled fast reactor applications [J]. Trans. Indian Inst. Met., 2010, 63: 151
doi: 10.1007/s12666-010-0021-1
[33] Karthik V, Murugan S, Parameswaran P, et al. Austenitic stainless steels for fast reactors-irradiation experiments, property evaluation and microstructural studies [J]. Energy Procedia, 2011, 7: 257
doi: 10.1016/j.egypro.2011.06.033
[34] Lai J K L, Chastell D J, Flewitt P E J. Precipitate phases in type 316 austenitic stainless steel resulting from long-term high temperature service [J]. Mater. Sci. Eng., 1981, 49: 19
doi: 10.1016/0025-5416(81)90129-4
[35] Vach M, Kuníková T, Dománková M, et al. Evolution of secondary phases in austenitic stainless steels during long-term exposures at 600, 650 and 800 oC [J]. Mater. Charact., 2008, 59: 1792
doi: 10.1016/j.matchar.2008.04.009
[36] Lv X L, Chen S H, Rong L J. Evolution of precipitate and its effect on the degradation of impact toughness in a carbon and nitrogen-controlled 316 stainless steel during thermal aging at 650 oC [J]. J. Mater. Res. Technol., 2024, 33: 3728
doi: 10.1016/j.jmrt.2024.10.043
[37] Xie A, Chen S H, Yin L C, et al. Microstructural evolution of the inner oxide layer of a Si-modified austenitic stainless steel exposed to oxygen-saturated lead-bismuth eutectic (LBE): Toward the origin of LBE penetration [J]. Corros. Sci., 2024, 237: 112350
doi: 10.1016/j.corsci.2024.112350
[38] Padilha A F, Escriba D M, Materna-Morris E, et al. Precipitation in AISI 316L(N) during creep tests at 550 and 600 oC up to 10 years [J]. J. Nucl. Mater., 2007, 362: 132
doi: 10.1016/j.jnucmat.2006.12.027
[39] Padilha A F, Rios P R. Decomposition of austenite in austenitic stainless steels [J]. ISIJ Int., 2002, 42: 325
doi: 10.2355/isijinternational.42.325
[40] Sourmail T. Precipitation in creep resistant austenitic stainless steels [J]. Mater. Sci. Technol., 2001, 17: 1
doi: 10.1179/026708301101508972
[41] The American Society of Mechanical Engineers. Boiler and pressure vessel code, section III: Rules for construction of nuclear power plant components, division 1, subsection NH: Class 1 components in elevated temperature service [S]. New York: ASME, 2015
[42] Zinkle S J. Radiation-induced effects on microstructure [A]. Comprehensive Nuclear Materials [M]. Amsterdam: Elsevier, 2012: 65
[43] Was G S. Irradiation-induced voids and bubbles [A]. Fundamentals of Radiation Materials Science: Metals and Alloys [M]. New York: Springer, 2017: 379
[44] Keown S R, Pickering F B. Niobium in stainless steels [A]. Proceedings of the International Symposium—Niobium 81 [C]. San Francisco, 1981: 1113
[45] Williams T M, Titchmarsh J M, Arkell D R. Void-swelling and precipitation in a neutron-irradiated, niobium-stabilised austenitic stainless steel [J]. J. Nucl. Mater., 1982, 107: 222
doi: 10.1016/0022-3115(82)90423-8
[46] Meng F M, Fu J Y. Modern Niobium Containing Stainless Steel [M]. Beijing: Metallurgical Industry Press, 2004: 1
[46] 孟繁茂, 付俊岩. 现代含铌不锈钢 [M]. 北京: 冶金工业出版社, 2004: 1
[47] Wang Q Y, Chen S H, Rong L J. δ-ferrite formation and its effect on the mechanical properties of heavy-section AISI 316 stainless steel casting [J]. Metall. Mater. Trans., 2020, 51A: 2998
[48] Wang Q Y, Chen S H, Lv X L, et al. Role of δ-ferrite in fatigue crack growth of AISI 316 austenitic stainless steel [J]. J. Mater. Sci. Technol., 2022, 114: 7
doi: 10.1016/j.jmst.2021.10.008
[49] Chen S H, Wang Q Y, Jiang H C, et al. Effect of δ-ferrite on hot deformation and recrystallization of 316KD austenitic stainless steel for sodium-cooled fast reactor application [J]. Acta Metall. Sin., 2024, 60: 367
[49] 陈胜虎, 王琪玉, 姜海昌 等. δ-铁素体对钠冷快堆用316KD奥氏体不锈钢热变形行为和动态再结晶的影响 [J]. 金属学报, 2024, 60: 367
doi: 10.11900/0412.1961.2022.00039
[50] Xie A, Chen S H, Chen S H, et al. Austenite decomposition behavior adjacent to δ-ferrite in a Si-modified Fe-Cr-Ni austenitic stainless steel during thermal aging at 550 oC [J]. Acta Mater., 2024, 272: 119948
doi: 10.1016/j.actamat.2024.119948
[51] Chen Y K, Wei S T, Wu D, et al. Mechanism of δ-ferrite decomposition in high Si-bearing austenitic stainless steel weld metal during aging at 550 oC [J]. Mater. Sci. Eng., 2023, A876: 145163
[52] Chen S H, Wang Q Y, Xie A, et al. Corrosion behavior of δ-ferrite in AISI 316 austenitic stainless steel exposed to oxygen-saturated lead-bismuth eutectic at 550 oC [J]. Mater. Charact., 2024, 211: 113930
doi: 10.1016/j.matchar.2024.113930
[53] de Bellefon G M, van Duysen J C, Sridharan K. Composition-dependence of stacking fault energy in austenitic stainless steels through linear regression with random intercepts [J]. J. Nucl. Mater., 2017, 492: 227
doi: 10.1016/j.jnucmat.2017.05.037
[54] Martinez L G, Imakuma K, Padilha A F. Influence of niobium on stacking-fault energy of all-austenite stainless steels [J]. Steel Res., 1992, 63: 221
[55] Lu S, Hu Q M, Johansson B, et al. Stacking fault energies of Mn, Co and Nb alloyed austenitic stainless steels [J]. Acta Mater., 2011, 59: 5728
doi: 10.1016/j.actamat.2011.05.049
[56] Xie A, Chen S H, Jiang H C, et al. Effects of Nb content and homogenization treatment on the microstructure and mechanical properties of cast austenitic stainless steel [J]. Acta Metall. Sin., 2025, 61: 1035
doi: 10.11900/0412.1961.2023.00249
[56] 谢 昂, 陈胜虎, 姜海昌 等. Nb含量和均质化处理对奥氏体不锈钢铸态组织和力学性能的影响 [J]. 金属学报, 2025, 61: 1035
[57] Wang J Q, Wu J R, Yao Z Q, et al. Mechanistic insights into the dual role of NbC in strength-toughness synergy of nuclear grade Fe-Ni-based alloys [J]. J. Mater. Res. Technol., 2025, 39: 6806
doi: 10.1016/j.jmrt.2025.11.041
[58] Zhang X, Li D Z, Li Y Y, et al. The influence of niobium on the plastic deformation behaviors of 310s austenitic stainless steel weld metals at different temperatures [J]. Mater. Sci. Eng., 2019, A743: 648
[59] Wu Y, Xie A, Chen S H, et al. Corrosion behavior of NbC and its effect on corrosion layer formation in liquid lead-bismuth eutectic of Nb-containing austenitic stainless steel [J]. Acta Metall. Sin., 2025, 61: 287
doi: 10.11900/0412.1961.2022.00650
[59] 吴 炀, 谢 昂, 陈胜虎 等. 含Nb奥氏体不锈钢中NbC的液态Pb-Bi共晶腐蚀行为及其对氧化层形成的影响 [J]. 金属学报, 2025, 61: 287
[60] Takechi H, Hasimoto S, Imagumbai M, translated by Fu J Y, Shang C J. How to Improve the Properties of Steel with Niobium: Production Technology of Niobium-Containing Steel [M]. Beijing: Metallurgical Industry Press, 2007: 1
[60] Takechi H, Hasimoto S, Imagumbai M著, 付俊岩, 尚成嘉译. 如何用铌改善钢的性能 : 含铌钢生产技术 [M]. 北京: 冶金工业出版社, 2007:1
[61] Akahori K, Maeno S, Kodama H, et al. Prediction of the formation region of eutectic NbC in a large 12Cr-Mo-V-Nb steel ingot [J]. Tetsu-to-Hagané, 1985, 71: 78
doi: 10.2355/tetsutohagane1955.71.1_78
[61] 赤堀 公彦, 前野 茂夫, 児玉 英世 等. 12Cr-Mo-V-Nb鋼大形鋼塊中の共晶NbCの発生領域の予測 [J]. 鉄と鋼, 1985, 71: 78
[62] Xie A, Chen S H, Wu Y, et al. Homogenization temperature dependent microstructural evolution and mechanical properties in a Nb-stabilized cast austenitic stainless steel [J]. Mater. Charact., 2022, 194: 112384
doi: 10.1016/j.matchar.2022.112384
[63] Nordberg H, Aronsson B. Solubility of niobium carbide in austenite [J]. J. Iron Steel Inst., 1968, 206: 1263
[64] Japan Society of Mechanical Engineers. Code for Nuclear Power Generation Facilities. Rules on Design and Construction for Nuclear Power Plants. Section II Fast Reactor Standards [S]. Tokyo: JSME, 2017
[64] 日本機械学会. 発電用原子力設備規格 設計⋅建設規格(2016年)第II編高速炉規格 [S]. 東京: 日本機械学会, 2017
[65] AFCEN. Design and Construction Rules for Mechanical Components of Nuclear Installations: High temperature research and fusion reactors [S]. RCC-MRx, 2015
[66] Solenthaler C, Ramesh M, Uggowitzer P J, et al. Precipitation strengthening of Nb-stabilized TP347 austenitic steel by a dispersion of secondary Nb(C,N) formed upon a short-term hardening heat treatment [J]. Mater. Sci. Eng., 2015, A647: 294
[67] Shin J H, Kim H S, Kong B S, et al. Development of thermo-mechanical processing to form high density of uniformly distributed nanosized carbides in austenitic stainless steels [J]. Mater. Sci. Eng., 2020, A775: 138986
[68] Shin J H, Kong B S, Eom H J, et al. Dynamic evolution of nanosized NbC precipitates in austenite matrix during deformation and its contribution to strengthening [J]. Mater. Sci. Eng., 2021, A806: 140816
[69] Zhao W X, Jiang S H, Liu W H, et al. Synergistic effects of microalloying and pre-straining on enhanced nanoprecipitation and creep property of alumina-forming austenitic stainless steels [J]. Mater. Sci. Eng., 2022, A857: 143995
[70] Mu R, Wang Y J, Song R B, et al. Constructing high-density dislocations by primary (Nb,Ti)(C,N) to induce massive secondary precipitations in austenitic heat-resistant cast steel [J]. Mater. Charact., 2024, 212: 113968
doi: 10.1016/j.matchar.2024.113968
[71] Ha V T, Jung W S, Suh J Y. Improved creep behavior of a high nitrogen Nb-stabilized 15Cr-15Ni austenitic stainless steel strengthened by multiple nanoprecipitates [J]. Metall. Mater. Trans., 2011, 42A: 3378
[72] Ha V T, Jung W S. Creep behavior and microstructure evolution at 750 oC in a new precipitation-strengthened heat-resistant austenitic stainless steel [J]. Mater. Sci. Eng., 2012, A558: 103
[73] Yang Y H, Zhu L H, Wang Q J, et al. Microstructural evolution and the effect on hardness and plasticity of S31042 heat-resistant steel during creep [J]. Mater. Sci. Eng., 2014, A608: 164
[74] Li Y M, Liu Y C, Liu C X, et al. Mechanism for the formation of Z-phase in 25Cr-20Ni-Nb-N austenitic stainless steel [J]. Mater. Lett., 2018, 233: 16
doi: 10.1016/j.matlet.2018.08.141
[75] Erneman J, Schwind M, Liu P, et al. Precipitation reactions caused by nitrogen uptake during service at high temperatures of a niobium stabilised austenitic stainless steel [J]. Acta Mater., 2004, 52: 4337
doi: 10.1016/j.actamat.2004.06.001
[76] Ding R G, Yan J, Li H Y, et al. Microstructural evolution of Alloy 709 during aging [J]. Mater. Charact., 2019, 154: 400
doi: 10.1016/j.matchar.2019.06.018
[77] Maziasz P J. Development of creep-resistant and oxidation-resistant austenitic stainless steels for high temperature applications [J]. JOM, 2018, 70: 66
doi: 10.1007/s11837-017-2642-x
[78] Zhou Y H, Liu Y C, Zhou X S, et al. Precipitation and hot deformation behavior of austenitic heat-resistant steels: A review [J]. J. Mater. Sci. Technol., 2017, 33: 1448
doi: 10.1016/j.jmst.2017.01.025
[79] Wang H T, Du H Y, Wei Y H, et al. Precipitation and properties at elevated temperature in austenitic heat-resistant steels—A review [J]. Steel Res. Int., 2021, 92: 2000378
doi: 10.1002/srin.v92.2
[80] Dalle F, Blat-Yrieix M, Dubiez-Le Goff S, et al. Conventional austenitic steels as out-of-core materials for Generation IV nuclear reactors [A]. Structural Materials for Generation IV Nuclear Reactors [M]. Amsterdam: Woodhead Publishing, 2017: 595
[81] Powell D J, Pilkington R, Miller D A. The precipitation characteristics of 20% Cr/25% Ni-Nb stabilised stainless steel [J]. Acta Metall., 1988, 36(3): 713
doi: 10.1016/0001-6160(88)90105-8
[82] Vaché N, Steyer P, Duret-Thual C, et al. Microstructural study of the NbC to G-phase transformation in HP-Nb alloys [J]. Materialia, 2020, 9: 100593
doi: 10.1016/j.mtla.2020.100593
[83] Zhang S Z, Shi X B, Su Y F, et al. G phase and ferrite in a high Si austenitic stainless steel during 510 oC aging [J]. Mater. Charact., 2024, 207: 113587
doi: 10.1016/j.matchar.2023.113587
[84] Su Y F, Zhang S Z, Jiao S X, et al. Microstructural stability of L12-strengthened Si-modified Fe-Cr-Ni alloy during 510-600 oC thermal aging [J]. J. Mater. Sci. Technol., 2026, 244: 246
doi: 10.1016/j.jmst.2025.05.013
[85] Chen Y K, Wu D, Li D Z, et al. Effects of stabilization heat treatment on microstructure and mechanical properties of Si-bearing 15Cr-9Ni-Nb austenitic stainless steel weld metal [J]. Acta Metall. Sin. (Engl. Lett.), 2023, 36: 637
doi: 10.1007/s40195-022-01497-1
[86] Hu G D, Wang P, Li D Z, et al. Precipitate evolution in a modified 25Cr-20Ni austenitic heat resistant stainless steel during creep rupture test at 750 oC [J]. Acta Metall. Sin., 2018, 54: 1705
[86] 胡国栋, 王 培, 李殿中 等. 新型25Cr-20Ni奥氏体耐热不锈钢750 ℃持久实验过程中析出相演变 [J]. 金属学报, 2018, 54: 1705
doi: 10.11900/0412.1961.2018.00361
[87] Perron A, Toffolon-Masclet C, Ledoux X, et al. Understanding sigma-phase precipitation in a stabilized austenitic stainless steel (316Nb) through complementary CALPHAD-based and experimental investigations [J]. Acta Mater., 2014, 79: 16
doi: 10.1016/j.actamat.2014.06.066
[88] Séran J L, Le Flem M. Irradiation-resistant austenitic steels as core materials for Generation IV nuclear reactors [A]. Structural Materials for Generation IV Nuclear Reactors [M]. Amsterdam: Woodhead Publishing, 2017: 285
[89] Kato T, Takahashi H, Izumiya M. Grain boundary segregation under electron irradiation in austenitic stainless steels modified with oversized elements [J]. J. Nucl. Mater., 1992, 189: 167
doi: 10.1016/0022-3115(92)90529-T
[90] Sakaguchi N, Watanabe S, Takahashi H. Effect of additional minor element on radiation-induced grain boundary segregation in austenitic stainless steel under electron irradiation [J]. Nucl. Instrum. Methods Phys. Res., 1999, 153B: 142
[91] Hackett M J, Busby J T, Miller M K, et al. Effects of oversized solutes on radiation-induced segregation in austenitic stainless steels [J]. J. Nucl. Mater., 2009, 389: 265
doi: 10.1016/j.jnucmat.2009.02.010
[92] Kawanishi H, Nodaka M, Sekimura N, et al. Effects of C and Nb additions to Fe-16Ni-15Cr alloy on void swelling [J]. J. Nucl. Mater., 1984, 122: 284
doi: 10.1016/0022-3115(84)90611-1
[93] Little E A. Development of radiation resistant materials for advanced nuclear power plant [J]. Mater. Sci. Technol., 2006, 22: 491
doi: 10.1179/174328406X90998
[94] Zinkle S J, Snead L L. Designing radiation resistance in materials for fusion energy [J]. Annu. Rev. Mater. Res., 2014, 44: 241
doi: 10.1146/matsci.2014.44.issue-1
[95] Shin J H, Kong B S, Jeong C, et al. Swelling resistance of an austenitic stainless steel with uniformly distributed nanosized NbC precipitates under heavy ion irradiation [J]. J. Nucl. Mater., 2022, 564: 153678
doi: 10.1016/j.jnucmat.2022.153678
[96] Shin J H, Kong B S, Jeong C, et al. Evaluation of radiation resistance of an austenitic stainless steel with nanosized carbide precipitates using heavy ion irradiation at 200 dpa [J]. Nucl. Eng. Technol., 2023, 55: 555
doi: 10.1016/j.net.2022.09.033
[97] Maziasz P J. Void swelling resistance of phosphorus-modified austenitic stainless steels during HFIR irradiation at 300-500 oC to 57 dpa [J]. J. Nucl. Mater., 1993, 200: 90
doi: 10.1016/0022-3115(93)90013-O
[98] Tanaka M P, Hamada S, Hishinuma A, et al. Microstructural development of austenitic stainless steels irradiated in HFIR [J]. J. Nucl. Mater., 1988, 155-157: 801
doi: 10.1016/0022-3115(88)90419-9
[99] Bozin S N, Rodchenkov B S, Kashtanov A D, et al. Study of construction materials for a lead-cooled reactor [J]. At. Energy, 2013, 113: 320
doi: 10.1007/s10512-013-9639-5
[100] Porollo S I, Shulepin S V, Konobeev Y V, et al. Influence of silicon on swelling and microstructure in Russian austenitic stainless steel EI-847 irradiated to high neutron doses [J]. J. Nucl. Mater., 2008, 378: 17
doi: 10.1016/j.jnucmat.2008.03.027
[101] Pakhomov I. BN-600 and BN-800 operating experience [R]. Russia, 2018
[102] Ashida T, Gondai Y, Inoue M, et al. Experimental reactor Joyo [A]. Sodium-Cooled Fast Reactors [M]. London: Academic Press, 2022: 9
[103] Shibahara I, Ukai S, Onose S, et al. Irradiation performance of modified 316 stainless steel for Monju fuel [J]. J. Nucl. Mater., 1993, 204: 131
doi: 10.1016/0022-3115(93)90209-H
[104] Sham T L, Wang Y L, Bass R, et al. A709 qualification plan update and mechanical properties data assessment [R]. Idaho Falls: Idaho National Laboratory, 2022
[105] Rupp R E, Wang Y, Zhang X, et al. Integrated FY-21 elevated-temperature mechanical-testing results for alloy 709 code case [R]. Idaho Falls: Idaho National Laboratory, 2021
[106] Sham T L, Natesan K. Code qualification plan for an advanced austenitic stainless steel, alloy 709, for sodium fast reactor structural applications [R]. Argonne: Argonne National Laboratory, 2017
[1] 张竟文, 余黎明, 刘晨曦, 丁然, 刘永长. 高Cr马氏体耐热钢的协同强化机制及形变热处理应用[J]. 金属学报, 2024, 60(6): 713-730.
[2] 王学, 于淑敏, 任遥遥, 刘洪, 刘洪伟, 胡磊. P92钢时效的Laves相演化行为[J]. 金属学报, 2014, 50(10): 1195-1202.
[3] 姚曼,高晓,曾维鹏,王旭东,徐海譞,Simon R. Phillpot. hcp-Ti中辐照诱发缺陷演化及温度效应的分子动力学研究[J]. 金属学报, 2013, 49(5): 530-536.
[4] 沙玉辉; 左良; 张静华; 徐永波; 胡壮麒 . 一种镍基单晶高温合金压缩蠕变强度的各向异性[J]. 金属学报, 2001, 37(11): 1142-1146 .