Please wait a minute...
金属学报  2024, Vol. 60 Issue (10): 1439-1450    DOI: 10.11900/0412.1961.2024.00143
  研究论文 本期目录 | 过刊浏览 |
超快激光诱导Cu薄膜熔化的神经网络分子动力学研究
高天雨1,2, 曾启昱1,2(), 陈博1,2, 康冬冬1,2, 戴佳钰1,2()
1 国防科技大学 理学院 长沙 410072
2 国防科技大学 湖南省极端条件物理及应用重点实验室 长沙 410072
Neural Network Molecular Dynamics Study of Ultrafast Laser-Induced Melting of Copper Nanofilms
GAO Tianyu1,2, ZENG Qiyu1,2(), CHEN Bo1,2, KANG Dongdong1,2, DAI Jiayu1,2()
1 College of Science, National University of Defense Technology, Changsha 410072, China
2 Hunan Key Laboratory of Extreme Matter and Applications, National University of Defense Technology, Changsha 410072, China
引用本文:

高天雨, 曾启昱, 陈博, 康冬冬, 戴佳钰. 超快激光诱导Cu薄膜熔化的神经网络分子动力学研究[J]. 金属学报, 2024, 60(10): 1439-1450.
Tianyu GAO, Qiyu ZENG, Bo CHEN, Dongdong KANG, Jiayu DAI. Neural Network Molecular Dynamics Study of Ultrafast Laser-Induced Melting of Copper Nanofilms[J]. Acta Metall Sin, 2024, 60(10): 1439-1450.

全文: PDF(1831 KB)   HTML
摘要: 

在飞秒激光作用下,材料将经历从凝聚态到高温高压状态、甚至是理想等离子体的剧烈结构转变。在理解这一过程的微观图像上,分子动力学模拟扮演着重要角色,但是对激光作用带来的激发态等问题,传统分子动力学描述存在原理上的困难。本工作结合温度依赖的神经网络原子间势能面与双温模型分子动力学方法,在量子精度下实现激光加热Cu薄膜的大尺度模拟,深入探讨了不同激光通量作用下的热力学状态时空演化与相变动力学,揭示了随着激光通量的增加,激光诱导的熔化动力学从非均匀熔化机制到均匀熔化机制发生转变的物理图像,为深入理解激光-物质相互作用过程提供了原子尺度的微观参考。

关键词 : 神经网络,  激光-物质相互作用,  熔化动力学,  双温模型    
Abstract:

Exploring ultrafast structural transitions in materials triggered by femtosecond laser pulses—from their condensed states to high-temperature, high-pressure conditions, and potentially to ideal plasmas—is a crucial scientific endeavor with profound implications for fields such as inertial confinement fusion, metal additive manufacturing, and laser processing. These extreme conditions, which are challenging to replicate and directly observe in experiments due to temporal and spatial resolution limitations, require theoretical models and simulations to decode the underlying microscopic mechanisms. Molecular dynamics (MD) simulations, especially when paired with advanced potential energy surfaces, are effective tools for addressing these challenges. However, maintaining a balance between computational efficiency and physical accuracy, particularly when simulating excited states induced by laser interactions, remains a formidable task. In this context, neural network potential energy surfaces (NNPES) have demonstrated exceptional capability for capturing the complex interactions and properties of materials under extreme conditions, providing vital links between quantum mechanics and macroscale phenomena. Using Cu as a prototypical example, the ability of NNPES to accurately depict lattice vibrations, thermophysical properties, and complex dynamics during laser-matter interactions has been demonstrated. By seamlessly integrating NNPES with a two-temperature MD model, this study directly simulates the atomic-scale dynamics of Cu thin films subjected to intense pulsed laser irradiation. This innovative approach, which combines quantum-level accuracy with large-scale thermodynamics and detailed microstructural evolution, provides unprecedented insights into the fundamental mechanisms of laser-induced melting. Our findings reveal two distinct melting behaviors in Cu, dependent on laser fluence. At fluences near the melting threshold, a heterogeneous melting process initiated at the film surface because of the lower free energy barrier was observed. The solid-liquid interface then moves inward at velocities of tens of meters per second, requiring hundreds of picoseconds for melting to complete. Conversely, at fluences well above the threshold, Cu films experience rapid and homogeneous melting, markedly different from conventional heating-induced melting. Here, the lattice temperature almost instantaneously exceeds the thermal stability limit, leading to uniform liquid nucleation and rapid growth throughout the film, culminating in complete melting within just tens of picoseconds. This study not only illuminates the atomic-scale dynamics of laser-induced melting but also underscores the transition from heterogeneous to homogeneous melting mechanisms as a function of laser fluence. This study serves as an invaluable research tool for enhancing our understanding of laser-matter interactions and their potential applications in optimizing laser-based manufacturing processes and predicting material behavior under extreme conditions. Moreover, the reliability and versatility of NNPES set the stage for extending the research to more complex systems, including alloys and amorphous materials. This expansion fosters robust connections between microscopic theories and macroscale applications, deepening our understanding of material responses to intense laser irradiation. Future studies employing this framework could explore complex physical phenomena such as explosive boiling and material disintegration during laser ablation, offering unique atomic-scale insights that could pave the way for groundbreaking discoveries and technological advancements.

Key words: neural network    laser-matter interaction    melting dynamics    two-temperature model
收稿日期: 2024-05-07     
ZTFLH:  O469  
基金资助:国家自然科学基金项目(12104507);湖南省科技创新领军人才项目(2021RC4026);湖南省研究生科研创新项目(CX20220070)
通讯作者: 戴佳钰,jydai@nudt.edu.cn,主要从事极端条件下物质科学研究;
曾启昱,zengqiyu@nudt.edu.cn,主要从事激光与物质相互作用的原子尺度模拟研究
Corresponding author: DAI Jiayu, professor, Tel: (0731)87001006, E-mail: jydai@nudt.edu.cn;
ZENG Qiyu, Tel: 18374847919, E-mail: zengqiyu@nudt.edu.cn
作者简介: 高天雨,男,1995年生,博士生
Iter.Lattice structureTime / psEnsemble typeTemperature / KPressure / GPaSampled configuration
0fcc0.5NPT30000
1fcc1NPT30000
2fcc2NPT30000
3fcc4NPT30000
4fcc8NPT30000
5fcc16NPT30005
6fcc4NVT200, 4007
7fcc16NVT200, 4001
8fcc2NVT50060
9fcc4NVT5005
10fcc16NVT50010
11fcc2NVT80013
12fcc4NVT8009
13fcc16NVT80060
14fcc2NVT1000, 1200, 150060
15fcc4NVT1000, 1200, 150060
16fcc16NVT1000, 1200, 150060
17fcc0.5NPT300021
18fcc1NPT300046
19fcc2NPT300060
20fcc4NPT300060
21fcc8NPT300060
22fcc16NVT30060
23fcc4NVT200, 40060
24fcc16NVT200, 40060
25fcc2NVT50060
26fcc4NVT50060
27fcc16NVT50060
28fcc2NVT80060
29fcc4NVT80060
30fcc16NVT80060
31fcc2NVT1000, 120060
32fcc4NVT1000, 120060
33fcc8NVT1000, 120060
34fcc, liquid2NVT1500, 2000, 250060, 60
35fcc, liquid4NVT1500, 2000, 250060, 60
36fcc, liquid8NVT1500, 2000, 250060, 60
37Liquid2NVT300060
表1  不同热力学条件下Cu深度势能(DP)模型的构型探索
图1  Cu的DP模型预测值和密度泛函理论(DFT)计算的能量、受力和Virial张量的对比
Itema0 / nmTm / KΔHm / (kJ·kg-1)εm / (kJ·kg-1)
Relative error / %1.120.390.520.40
DP result0.36551275 ± 25232.3 ± 11.2658.7 ± 49.1
Experiment result0.3615[48]1280[51]231.1[53]661.3[51,53-56]
表2  使用DP模型得到的Cu的晶格常数(a0)、熔点(Tm)、相变潜热(ΔHm)、熔化阈值(εm)及其与实验值[48,51,53~56]的对比
图2  温度为300 K时Cu声子谱的DP模型结果与实验结果[49]对比
图3  不同压强条件下Cu熔点的DP模型结果与实验结果[51]对比
图4  Cu的晶格比热容(cp )和电子比热容(ce)
图5  18 mJ/cm2激光通量下Cu薄膜的演化动力学过程
图6  30 mJ/cm2激光通量下Cu薄膜的演化动力学过程
1 Abu-Shawareb H, Acree R, Adams P, et al. Lawson criterion for ignition exceeded in an inertial fusion experiment [J]. Phys. Rev. Lett., 2022, 129: 075001
2 Shugaev M V, Wu C P, Armbruster O, et al. Fundamentals of ultrafast laser-material interaction [J]. MRS Bull., 2016, 41: 960
3 Roy N K, Dibua O G, Jou W, et al. A comprehensive study of the sintering of copper nanoparticles using femtosecond, nanosecond, and continuous wave lasers [J]. J. Micro Nano-Manuf., 2018, 6: 010903
4 Cheng C W, Chang C L, Chen J K, et al. Femtosecond laser melting of silver nanoparticles: Comparison of model simulations and experimental results [J]. Appl. Phys., 2018, 124A: 371
5 Zhang H, Li C, Bevillon E, et al. Ultrafast destructuring of laser-irradiated tungsten: Thermal or nonthermal process [J]. Phys. Rev., 2016, 94B: 224103
6 Chen Z, Mo M, Soulard L, et al. Interatomic potential in the nonequilibrium warm dense matter regime [J]. Phys. Rev. Lett., 2018, 121: 075002
7 Ernstorfer R, Harb M, Hebeisen C T, et al. The formation of warm dense matter: Experimental evidence for electronic bond hardening in gold [J]. Science, 2009, 323: 1033
doi: 10.1126/science.1162697 pmid: 19164708
8 Mo M Z, Chen Z, Li R K, et al. Heterogeneous to homogeneous melting transition visualized with ultrafast electron diffraction [J]. Science, 2018, 360: 1451
doi: 10.1126/science.aar2058 pmid: 29954977
9 Mo M Z, Murphy S, Chen Z J, et al. Visualization of ultrafast melting initiated from radiation-driven defects in solids [J]. Sci. Adv., 2019, 5: eaaw0392
10 Wu J, Tang M X, Zhao L R, et al. Ultrafast atomic view of laser-induced melting and breathing motion of metallic liquid clusters with MeV ultrafast electron diffraction [J]. Proc. Natl. Acad. Sci. USA, 2022, 119: e2111949119
11 Mahieu B, Jourdain N, Ta Phuoc K, et al. Probing warm dense matter using femtosecond X-ray absorption spectroscopy with a laser-produced betatron source [J]. Nat. Commun., 2018, 9: 3276
doi: 10.1038/s41467-018-05791-4 pmid: 30115918
12 Jourdain N, Lecherbourg L, Recoules V, et al. Ultrafast thermal melting in nonequilibrium warm dense copper [J]. Phys. Rev. Lett., 2021, 126: 065001
13 Chen Z, Curry C B, Zhang R, et al. Ultrafast multi-cycle terahertz measurements of the electrical conductivity in strongly excited solids [J]. Nat. Commun., 2021, 12: 1638
doi: 10.1038/s41467-021-21756-6 pmid: 33712576
14 Hohlfeld J, Wellershoff S S, Güdde J, et al. Electron and lattice dynamics following optical excitation of metals [J]. Chem. Phys., 2000, 251: 237
15 Lin Z B, Zhigilei L V. Thermal excitation of d band electrons in Au: Implications for laser-induced phase transformations [A]. Proceedings of SPIE 6261, High-Power Laser Ablation VI [C]. Taos: SPIE, 2006: 62610U
16 Lin Z B, Zhigilei L V, Celli V. Electron-phonon coupling and electron heat capacity of metals under conditions of strong electron-phonon nonequilibrium [J]. Phys. Rev., 2008, 77B: 075133
17 Lee J W, Kim M, Kang G, et al. Investigation of nonequilibrium electronic dynamics of warm dense copper with femtosecond X-ray absorption spectroscopy [J]. Phys. Rev. Lett., 2021, 127: 175003
18 Grolleau A, Dorchies F, Jourdain N, et al. Femtosecond resolution of the nonballistic electron energy transport in warm dense copper [J]. Phys. Rev. Lett., 2021, 127: 275901
19 Lin Z B, Zhigilei L V. Time-resolved diffraction profiles and atomic dynamics in short-pulse laser-induced structural transformations: Molecular dynamics study [J]. Phys. Rev., 2006, 73B: 184113
20 Molina J M, White T G. A molecular dynamics study of laser-excited gold [J]. Matter Radiat. Extremes, 2022, 7: 036901
21 Ivanov D S, Zhigilei L V. Effect of pressure relaxation on the mechanisms of short-pulse laser melting [J]. Phys. Rev. Lett., 2003, 91: 105701
22 Daraszewicz S L, Giret Y, Naruse N, et al. Structural dynamics of laser-irradiated gold nanofilms [J]. Phys. Rev., 2013, 88B: 184101
23 Murphy S T, Daraszewicz S L, Giret Y, et al. Dynamical simulations of an electronically induced solid-solid phase transformation in tungsten [J]. Phys. Rev., 2015, 92B: 134110
24 Murphy S T, Giret Y, Daraszewicz S L, et al. Contribution of electronic excitation to the structural evolution of ultrafast laser-irradiated tungsten nanofilms [J]. Phys. Rev., 2016, 93B: 104105
25 Arefev M I, Shugaev M V, Zhigilei L V. Kinetics of laser-induced melting of thin gold film: How slow can it get? [J]. Sci. Adv., 2022, 8: eabo2621
26 Behler J, Parrinello M. Generalized neural-network representation of high-dimensional potential-energy surfaces [J]. Phys. Rev. Lett., 2007, 98: 146401
27 Zhang L F, Han J Q, Wang H, et al. Deep potential molecular dynamics: A scalable model with the accuracy of quantum mechanics [J]. Phys. Rev. Lett., 2018, 120: 143001
28 Zeng Q Y, Chen B, Yu X X, et al. Towards large-scale and spatiotemporally resolved diagnosis of electronic density of states by deep learning [J]. Phys. Rev., 2022, 105B: 174109
29 Zeng Q Y, Yu X X, Yao Y P, et al. Ab initio validation on the connection between atomistic and hydrodynamic description to unravel the ion dynamics of warm dense matter [J]. Phys. Rev. Res., 2021, 3: 033116
30 Yang F H, Zeng Q Y, Chen B, et al. Lattice thermal conductivity of MgSiO3 perovskite and post-perovskite under lower mantle conditions calculated by deep potential molecular dynamics [J]. Chin. Phys. Lett., 2022, 39: 116301
31 Niu H Y, Bonati L, Piaggi P M, et al. Ab initio phase diagram and nucleation of gallium [J]. Nat. Commun., 2020, 11: 2654
doi: 10.1038/s41467-020-16372-9 pmid: 32461573
32 Santos-Florez P A, Yanxon H, Kang B, et al. Size-dependent nucleation in crystal phase transition from machine learning metadynamics [J]. Phys. Rev. Lett., 2022, 129: 185701
33 Chen B, Zeng Q Y, Yu X X, et al. Three-step formation of diamonds in shock-compressed hydrocarbons: Decomposition, species separation, and nucleation [J]. arXiv: 2208. 01830, 2022
34 Chen B, Zeng Q Y, Wang H, et al. Atomistic mechanism of phase transition in shock compressed gold revealed by deep potential [J]. arXiv: 2006. 13136, 2021
35 Qiu R, Zeng Q Y, Wang H, et al. Anomalous thermal transport across the superionic transition in ice [J]. Chin. Phys. Lett., 2023, 40: 116301
36 Zeng Q Y, Chen B, Zhang S, et al. Full-scale ab initio simulations of laser-driven atomistic dynamics [J]. npj Comput. Mater., 2023, 9: 213
37 Wang H, Zhang L F, Han J Q, et al. DeePMD-kit: A deep learning package for many-body potential energy representation and molecular dynamics [J]. Comput. Phys. Commun., 2018, 228: 178
38 Zhang L F, Lin D Y, Wang H, et al. Active learning of uniformly accurate interatomic potentials for materials simulation [J]. Phys. Rev. Mater., 2019, 3: 023804
39 Zhang Y Z, Gao C, Liu Q R, et al. Warm dense matter simulation via electron temperature dependent deep potential molecular dynamics [J]. Phys. Plasmas, 2020, 27: 122704
40 Zeng Q Y, Dai J Y. Structural transition dynamics of the formation of warm dense gold: From an atomic scale view [J]. Sci. China Phys. Mech. Astron., 2020, 63: 263011
41 Dai J Y, Hou Y, Yuan J M. Unified first principles description from warm dense matter to ideal ionized gas plasma: Electron-ion collisions induced friction [J]. Phys. Rev. Lett., 2010, 104: 245001
42 Dai J Y, Kang D D, Zhao Z X, et al. Dynamic ionic clusters with flowing electron bubbles from warm to hot dense iron along the hugoniot curve [J]. Phys. Rev. Lett., 2012, 109: 175701
43 Kresse G, Furthmüller J. Efficient iterative schemes for ab initio total-energy calculations using a plane-wave basis set [J]. Phys. Rev., 1996, 54B: 11169
44 Perdew J P, Burke K, Ernzerhof M. Generalized gradient approximation made simple [J]. Phys. Rev. Lett., 1996, 77: 3865
doi: 10.1103/PhysRevLett.77.3865 pmid: 10062328
45 Blöchl P E. Projector augmented-wave method [J]. Phys. Rev., 1994, 50B: 17953
46 Ivanov D S, Zhigilei L V. Combined atomistic-continuum modeling of short-pulse laser melting and disintegration of metal films [J]. Phys. Rev., 2003, 68B: 064114
47 Plimpton S. Fast parallel algorithms for short-range molecular dynamics [J]. J. Comput. Phys., 1995, 117: 1
48 Kittel C. Kittel's Introduction to Solid State Physic [M]. Beijing: Machine Press, 2020: 86
49 Tadano T, Gohda Y, Tsuneyuki S. Anharmonic force constants extracted from first-principles molecular dynamics: Applications to heat transfer simulations [J]. J. Phys.: Condens. Matter., 2014, 26: 225402
50 Nilsson G, Rolandson S. Lattice dynamics of copper at 80 K [J]. Phys. Rev., 1973, 7B: 2393
51 Japel S, Schwager B, Boehler R, et al. Melting of copper and nickel at high pressure: The role of d electrons [J]. Phys. Rev. Lett., 2005, 95: 167801
52 Simon F, Glatzel G. Bemerkungen zur schmelzdruckkurve [J]. Z. Anorg. Allg. Chem., 1929, 178: 309
53 Cagran C, Wilthan B, Pottlacher G. Enthalpy heat of fusion and specific electrical resistivity of pure silver, pure copper and the binary Ag-28Cu alloy [J]. Thermochim. Acta, 2006, 445: 104
54 Nizomov Z, Saidov R H, Gulov B N, et al. Temperature dependence of the heat capacity of aluminium, copper, silicon, magnesium, zinc and comparison with Debye theory [J]. Interconf, 2021, 55: 307
55 Smirnov N A. Copper, gold, and platinum under femtosecond irradiation: Results of first-principles calculations [J]. Phys. Rev., 2020, 101B: 094103
56 Cho B I, Ogitsu T, Engelhorn K, et al. Measurement of electron-ion relaxation in warm dense copper [J]. Sci. Rep., 2016, 6: 18843
doi: 10.1038/srep18843 pmid: 26733236
57 Hohlfeld J, Müller J G, Wellershoff S S, et al. Time-resolved thermoreflectivity of thin gold films and its dependence on film thickness [J]. Appl. Phys., 1997, 64B: 387
58 Zhang Y W, Chen J K. Ultrafast melting and resolidification of gold particle irradiated by pico- to femtosecond lasers [J]. J. Appl. Phys., 2008, 104: 054910
[1] 文通其, 刘怀忆, 龚小国, 叶贝琳, 刘思宇, 李卓远. 深度势能方法在材料科学中的应用[J]. 金属学报, 2024, 60(10): 1299-1311.
[2] 冀秀梅, 侯美伶, 王龙, 刘玠, 高克伟. 基于机器学习的中厚板变形抗力模型建模与应用[J]. 金属学报, 2023, 59(3): 435-446.
[3] 余滨杉,王社良,杨涛,樊禹江. 基于遗传算法优化的SMABP神经网络本构模型[J]. 金属学报, 2017, 53(2): 248-256.
[4] 侯介山,周兰章,郭建亭,袁超. NiAl合金超塑性的人工神经网络预测[J]. 金属学报, 2013, 49(11): 1333-1338.
[5] 余晖 KIM Youngmin 于化顺 YOU Bongsun 闵光辉. Mg-Zn-Zr-Ce合金高温变形行为与热加工性能研究[J]. 金属学报, 2012, 48(9): 1123-1131.
[6] 邓天勇 吴迪 许云波 赵彦峰 刘相华 王国栋. 普碳钢中厚板热轧温度制定的一种新的数学方法[J]. 金属学报, 2009, 45(1): 67-72.
[7] 吴令; 姜周华; 龚伟; 梁连科 . 遗传神经网络改进正规溶液模型及其在二元渣系中的应用[J]. 金属学报, 2008, 44(7): 799-802 .
[8] 连利仙; 刘颖; 叶金文; 高升吉; 涂铭旌 . 基于人工神经网络的Nd-Fe-Co-Zr-B系永磁合金磁性能的预测模型[J]. 金属学报, 2005, 41(5): 529-533 .
[9] 李军伟; 彭志方 . 用人工神经网络法预测镍基单晶高温合金的蠕变断裂寿命[J]. 金属学报, 2004, 40(3): 257-262 .
[10] 由伟; 白秉哲; 方鸿生 ; 谢锡善 . 用人工神经网络模型预测钢的奥氏体形成温度[J]. 金属学报, 2004, 40(11): 1133-1137 .
[11] 李新城; 陈光; 朱伟兴; 王匀; 张开华; 汪建敏 . 齿轮选材及热处理工艺智能专家系统[J]. 金属学报, 2004, 40(10): 1051-1054 .
[12] 骆宇时; 彭志方 . 镍基高温合金中γ’和γ相点阵常数的简捷人工神经网络预测法[J]. 金属学报, 2003, 39(9): 897-902 .
[13] 李锋军; 沈厚发; 柳百成 . 消失模铸造充型过程的模拟方法[J]. 金属学报, 2003, 39(7): 686-690 .
[14] 由伟; 方鸿生; 白秉哲 . 用反向传播人工神经网络预测低碳低合金钢的马氏体转变开始温度[J]. 金属学报, 2003, 39(6): 630-634 .