金属学报, 2022, 58(11): 1441-1458 DOI: 10.11900/0412.1961.2022.00322

综述

高熵合金跨尺度异构强韧化及其力学性能研究进展

安子冰1, 毛圣成,1, 张泽1,2, 韩晓东,1

1.北京工业大学 材料与制造学部 固体微结构与性能研究所 北京 100124

2.浙江大学 材料科学与工程学院 杭州 310058

Strengthening-Toughening Mechanism and Mechanical Properties of Span-Scale Heterostructure High-Entropy Alloy

AN Zibing1, MAO Shengcheng,1, ZHANG Ze1,2, HAN Xiaodong,1

1.Institute of Microstructure and Properties of Advanced Materials, Faculty of Materials and Manufacturing, Beijing University of Technology, Beijing 100124, China

2.Department of Materials Science and Engineering, Zhejiang University, Hangzhou 310058, China

通讯作者: 毛圣成,scmao@bjut.edu.cn,主要从事透射电镜原位技术开发及其在高温合金、高熵合金中的应用;韩晓东,xdhan@bjut.edu.cn,主要从事高空间分辨原位显微学技术及科学装置研发及金属材料塑性变形行为研究

责任编辑: 李海兰

收稿日期: 2022-07-04   修回日期: 2022-08-03  

基金资助: 国家重点研发计划项目(2021YFA1200201)
国家自然科学基金项目(52071003)
国家自然科学基金项目(91860202)
国家自然科学基金项目(51988101)
北京市科技新星计划交叉学科合作课题项目(Z211100002121170)
北京学者项目(PXM2020_014204_000021)
高等学校学科创新引智计划(111计划)项目(DB18015)

Corresponding authors: MAO Shengcheng, professor, Tel:(010)67396769, E-mail:scmao@bjut.edu.cn;HAN Xiaodong, professor, Tel:(010)67392281, E-mail:xdhan@bjut.edu.cn

Received: 2022-07-04   Revised: 2022-08-03  

Fund supported: National Key Research and Development Program of China(2021YFA1200201)
National Natural Science Foundation of China(52071003)
National Natural Science Foundation of China(91860202)
National Natural Science Foundation of China(51988101)
Interdisciplinary Cooperation Project of Beijing Science and Technology Nova Program(Z211100002121170)
Beijing Municipal Education Commission Project(PXM2020_014204_000021)
Discipline Innovation and Talent Introduction Program in Colleges and Universities(DB18015)

作者简介 About authors

安子冰,男,1993年生,博士

摘要

高熵合金突破了传统合金设计理念的桎梏,具有高强度、高硬度、高耐磨性及抗腐蚀性,是一种具有巨大发展前景的新型金属材料。然而,金属材料的强度与塑性之间存在倒置矛盾关系,高熵合金仍受困于这一难题。因此,设计开发兼具高强度与高塑性的高熵合金材料已成为目前研究热点与难点。近年来,异构设计理念在传统金属材料强韧化这一问题上得到发展,如何设计异构高熵合金以实现高熵合金强韧化,使合金兼具高强度与高塑性,引起了科研人员的重视。本文从异构显微组织尺度出发,综述了目前存在的异构显微结构设计方法,分析了不同异构组织对其强韧化机制及力学性能的影响,并对未来高强韧高熵合金显微结构设计进行了展望。

关键词: 高熵合金; 异构; 强韧化; 力学性能

Abstract

High-entropy alloys overcome the limitations posed by traditional alloys due to features such as high strength, toughness, high wear resistance, and corrosion resistance. These alloys are novel metallic materials with excellent application potential; however, typically an inverse relationship is observed between the strength and ductility of a metal, which includes high-entropy alloys. Therefore, the design and development of high entropy alloys with high strength and high ductility have become a limitation in current research. Recently, heterostructure design has achieved great success in strengthening and toughening traditional metallic materials. Heterostructured and high-entropy alloys has garnered much attention and research interest to realize the strength and toughness of high-entropy alloys with high strength and high ductility. This study reviews the existing design models for heterostructures from the heterostructure scale perspective. Furthermore, the effects of different heterostructures on the strengthening and toughening mechanism and mechanical properties were analyzed, and future microstructural designs with high strength and toughness were anticipated.

Keywords: high-entropy alloy; heterostructure; strengthening and toughening; mechanical property

PDF (7106KB) 元数据 多维度评价 相关文章 导出 EndNote| Ris| Bibtex  收藏本文

本文引用格式

安子冰, 毛圣成, 张泽, 韩晓东. 高熵合金跨尺度异构强韧化及其力学性能研究进展[J]. 金属学报, 2022, 58(11): 1441-1458 DOI:10.11900/0412.1961.2022.00322

AN Zibing, MAO Shengcheng, ZHANG Ze, HAN Xiaodong. Strengthening-Toughening Mechanism and Mechanical Properties of Span-Scale Heterostructure High-Entropy Alloy[J]. Acta Metallurgica Sinica, 2022, 58(11): 1441-1458 DOI:10.11900/0412.1961.2022.00322

高性能金属材料作为结构材料被广泛应用于交通运输、国防装备、航空航天等各个领域,开发兼具高强度与高塑性(高强韧)的金属材料是应对使役条件日益严苛的重要途径。传统合金通常以1种或2种元素作为主要元素,如钛合金[1,2]、镁合金[3]、铝合金[4]及钢材[5]等,并添加少量或微量其他改性元素来优化其力学、物理、化学性能。传统合金设计首要考虑的是如何避免对力学性能有害的金属间化合物形成。因此,传统合金中改性元素种类有限且含量一般控制在较低水平,进而限制了其成分调控范围、固溶强化效果和合金性能。2004年,Yeh等[6]和Cantor等[7]独立提出了多主元合金设计理念。不同于传统金属材料设计,该设计理念通过增加合金组元数来提高材料的构型熵,从而获得稳定的固溶体结构,避免形成金属间化合物,此类合金又称为多主元合金或者高熵合金。

高熵合金通常由5种及以上元素按等原子比或近等原子比组成,每种元素占比可在5%~35% (原子分数,下同)范围内调整,合金混合熵(ΔS)一般大于等于1.5R (R为理想气体常数)[8]。随着高熵合金研究的发展,高熵合金的定义也逐渐宽泛,人们将含有4种元素或者其中某一种元素含量低于5%或者高于35%的合金也称为高熵合金[9,10]。相较于传统合金,高熵合金具有4个特殊效应:高熵效应、晶格畸变效应、缓滞扩散效应和“鸡尾酒效应”[8]。高熵合金所具有的四大效应使其具有多种优良性能,例如:优异的力学性能[11]、良好的热稳定性[12]、抗腐蚀[13]、抗摩擦性[14]等,展示出巨大的发展前景。

高熵合金的初期研究主要集中于化学成分设计以及相结构预测[15~19],研究者力图通过改变合金化学成分组成调控合金的显微组织,从而获得具有优异力学性能的高熵合金材料。fcc和bcc结构是高熵合金典型的晶体结构。其中,bcc结构高熵合金通常由Hf、Nb、Ta、Ti、Zr、W、Mo等难熔元素组成,因此又被称为难熔高熵合金[20,21]。难熔高熵合金具有优异的高低温屈服强度,但面临室温拉伸塑性差的难题,而制约了其室温的加工和应用。例如,HfTaTiZr难熔高熵合金室温拉伸屈服强度为1.5 GPa,但其拉伸塑性仅为3%[22]。fcc结构高熵合金通常由Co、Cr、Ni、Fe、Mn、Al等元素组成。其中,CoCrFeNi、CoCrFeNiMn、Al0.3CoCrFeNi是研究最广泛的高熵合金。与bcc高熵合金高强度低塑性的力学性能相反,fcc高熵合金呈现出低强度高塑性的力学性能[23,24]。fcc高熵合金一般具有较好的可加工性,因此,可以运用细晶强化[25~27]、第二相析出强化[28~30]、位错强化[31]、孪晶强化[32,33]等方式提高其强度。然而,在提升fcc高熵合金强度的同时,不可避免地会降低其塑性,呈现出强度-塑性倒置的矛盾关系。

为解决高熵合金中强度-塑性倒置关系,获得高强韧高熵合金材料,研究者提出了系列平衡材料强度与塑性的设计理念,包括:韧性纳米析出强化[34]、共晶[35]、孪晶/相变诱导塑性变形[36]等。该系列合金设计理念在显微结构上具有共性特征:非均匀显微结构,即异质结构(简称异构)[37]。高熵合金中的异构还包括:局部化学成分波动[38]、中/短程有序结构[39,40]、梯度晶粒结构[41]、梯度纳米孪晶结构[42]、双峰结构[43]、层片结构[44]以及多相结构[34]等。高熵合金的异构化已被证明是解决强度-塑性倒置的重要途径[45],如图1[25,34,43,46~48]所示。异构高熵合金实现材料强度和塑性同步提升的关键在于其异质界面结构。在变形过程中,异质界面两侧存在应变梯度,从而激发几何必需位错在异构界面上堆积协调应变差,产生异构变形诱导强化与硬化机制,进而极大提高了合金的加工硬化能力,最终实现强度和塑性的同步提高[45]。因此,在高熵合金优异的固溶强化基础之上,结合显微组织设计,构建和发展新型异质结构是获得优异力学性能的重要途径。

图1

图1   异构高熵合金与传统合金以及均质高熵合金材料的强度-塑性对比[25,34,43,46~48]

Fig.1   Comparison of strength and ductility of high-entropy alloys (HEAs) with other conventional alloys and homogeneous HEAs[25,34,43,46~48]


本文将着重介绍高熵合金跨尺度异构显微结构设计、变形机制、强韧化机理及其力学性能,期望为发展新型高强韧异构高熵合金显微结构设计提供新思路。

1 原子尺度异构强韧化

理论上,高熵合金内各元素分布高度混乱,其晶格点阵位置被不同的元素占据,不同位置的元素排列在统计上呈现出明显的不均匀性,是一种典型的原子尺度异构材料[37]。Ding等[38]利用球差校正透射电镜(aberration-corrected transmission electron microscopy)揭示了高熵合金中元素的原子尺度分布,从实验上给出了原子尺度异构的直观证据。图2a和b[38]为CoCrFeNiMn合金的原子尺度扫描透射电镜高角环形暗场(high-angle annular dark field scanning transmission electron microscopy,HAADF-STEM)像。从图中可以看出,5种元素在原子尺度的分布呈现异构特征。各元素的线分布(图2c[38])进一步证实了元素在原子尺度的波动行为。原子尺度异构可产生较大的晶格应变,从而提高合金的固溶强化效果。因此,相比于传统金属材料,高熵合金具有较高的本征屈服强度(高晶格摩擦力)。这种由原子尺度异构引起的固溶强化效果在bcc结构高熵合金中体现得更为明显,这是由于bcc结构高熵合金组成元素具有更大的原子半径差[49~51]。如图2f[49]所示,HfNbTaTiV难熔高熵合金展示出了较大的晶格间距波动,表明其具有较高的晶格畸变效应。力学性能测试表明,该合金屈服强度高达1350 MPa,同时具有较高的压缩塑性(> 45%),屈服强度远超其他高熵合金材料。

图2

图2   CoCrFeNiMn、CoCrFeNiPd[38]和HfNbTaTiV[49]高熵合金成分分布与力学性能

Fig.2   Chemical distribution and mechanical properties of CoCrFeNiMn, CoCrFeNiPd[38], and HfNbTaTiV[49] HEAs

(a) atomic-resolution chemical distribution of CoCrFeNiMn alloy

(b) atomic-resolution chemical distribution of CoCrFeNiPd alloy

(c) chemical distribution line scan of CoCrFeNiMn and CoCrFeNiPd alloys

(d) high-angle annular dark field scanning transmission electron microscopy (HAADF-STEM) image of CoCrFeNiPd alloys and lattice strain distribution (Inset is the SAED pattern)

(e) tensile mechanical properties of CoCrFeNiMn, CoCrFeNiPd alloys and compared with other alloys

(f) lattice distortion analysis and compressive properties of HfNbTaTiV alloy


2 纳米尺度异构强韧化

2.1 局部化学成分波动异构

高熵合金组成元素原子半径及原子间结合力的差异化导致合金元素分布不均匀,产生局部化学成分波动(local chemical fluctuation,LCF)[52~54]。通过调控高熵合金原子半径差、电负性差以及混合焓大小,可以提升高熵合金的成分不均匀性,从而形成1~3 nm尺寸的局部成分波动(图2b[38])。因此,高熵合金元素分布不再是高度无序的固溶体结构,而是形成了具有局部化学成分波动的异构高熵合金材料。如图2a~c[38]所示,相较于CoCrFeNiMn高熵合金,LCF在CoCrFeNiPd高熵合金分布更明显,这是由于Pd元素具有较大的原子半径及电负性,提高其形成金属间化合物的趋势,从而产生更明显的成分波动[17,38,55]。与CoCrFeNiMn高熵合金对比,CoCrFeNiPd合金在塑性变形过程中,LCF的存在增强了对位错运动的阻碍作用,促使位错发生交滑移,提升了位错之间的交互作用,提高了材料的加工硬化能力,从而有效提高材料的强度与塑性(图2e[38])。

此外,Lei等[56]在HfNbTiZr难熔高熵合金中加入O原子,形成有序的氧复合物结构(ordered oxygen complexes,OOCs),从而构筑了纳米级异质结构。利用三维原子探针及球差矫正透射电镜技术,阐明了OOCs的化学成分组成、尺寸及分布情况。研究表明,O元素更容易和Zr、Ti元素形成氧复合物,其尺寸在1~3 nm (图3a[56])。通过对变形后样品显微组织分析可知,OOCs的存在改变了位错的滑移方式,由传统的平面滑移转变为交滑移为主的塑性变形方式(图3b[56]),从而产生了波状位错墙,极大地提高了位错密度,产生了明显的加工硬化行为,提升了材料的拉伸塑性(图3a[56])[57]。与此同时,在变形过程中,OOCs可以有效地阻碍位错运动,提高位错运动的阻力,从而产生明显的强化效应,使得该合金具有较高的强度。最终该合金实现了高屈服强度(1100 MPa)与高拉伸塑性(27.7%)的完美结合,如图3c[56]所示。此外,该异构合金的成功也颠覆了人们对氧复合物的认知,一般认为O元素的加入会导致合金脆化,而有效构筑OCCs异质结构,不仅可以提高合金强度同时还能提升合金塑性,为新型高熵合金显微结构设计提供新思路。难熔高熵合金由于拉伸塑性较差,通过热机械处理调控合金显微结构改善合金力学性能的方式不再适用,文献[56]中的LCF异构显微结构设计思路为提高难熔合金力学性能提供新角度。因此,在未来的研究中,可以尝试通过调控LCF尺寸、三维分布以及密度,实现进一步提升难熔高熵合金力学性能的目标。

图3

图3   (HfNbTiZr)98O2高熵合金显微结构及力学性能[56]

Fig.3   Microstructure and mechanical properties of (HfNbTiZr)98O2 high-entropy alloy[56] (O-2 represents (TiZrHfNb)98O2, and N-2 represents (TiZrHfNb)98N2)

(a) atom probe tomography image and the O composition profile as a function of the distance to the interface for a selection of particles (left axis) and evolution of the composition of the main constituents relative to their respective matrix composition (right axis) (Ni is the number of the ith atom, while Ci and Ci, matrix are the concentrations of the ith atom in the ordered oxygen complexes (OOCs) and in the matrix, respectively; and the inset shows a close-up of one OOC)

(b) TEM image of O-2 HEA at 8% tensile strain (The red arrows indicate the dipolar walls)

(c) tensile mechanical properties of the (HfNbTiZr)98O2 alloy and compared alloys (σy is the yield strength (squares), σUTS is the ultimate strength (diamonds), and ε is the elongation (circles). The inset shows the corresponding strain-hardening response (dσ/dε))


2.2 中/短程有序异构

相较于局部化学成分波动,短程有序(short-range-ordering,SRO)结构是一种更小尺度的异质结构,其广泛存在于高熵合金中并影响高熵合金力学性能[58~63]。短程有序是由于合金元素之间结合焓不同而导致的化学元素有序排列现象。由于原子分辨元素分布图(atomic resolution chemical mapping)实验具有很大的挑战性,导致短程有序结构很难在实验中观察到,因此,早期短程有序结构研究多为模拟实验。Li等[60]通过对CoCrNi合金原子尺度模拟实验表明SRO的存在提高了位错激活能,改变了局部层错能,造成能量的波动,从而导致位错难以启动。其次,材料局部层错能的变化导致材料塑性变形方式的改变。一般地,晶体材料塑性变形可以通过位错滑移、层错、孪晶及相变等方式实现,而这些变形方式的选择与材料层错能密切相关。这是由于材料的层错能较低时(SFE < 50 mJ/m2),不全位错滑移产生宽度较大的扩展位错,滑移过程中很难束集,因此阻碍了全位错交滑移,此时材料变形主要由不全位错主导,即发生孪晶变形[64]。此外,SRO的存在也会造成局部晶格畸变增加,提高位错运动的阻力,从而产生强化效果。随着先进表征技术的发展,Zhang等[65]通过TEM能量过滤衍射技术在时效处理的CoCrNi合金中实现了SRO的实验观察(图4a~e[65]),揭示了SRO的尺寸(1.13 nm)及分布密度。同时,相比于没有SRO的CoCrNi合金,力学实验研究表明,SRO的存在提高了合金的屈服强度及断裂强度。更为重要的是,合金的初始加工硬化率提升了1倍,如图4f~i[65]所示。通过对变形后样品位错组态分析表明,SRO的存在使得位错更容易进行平面滑移。这是由于初始位错滑移过后,打破了原来的原子排列顺序,破坏了SRO结构,产生滑移面软化现象,从而抑制了位错交滑移,促进位错平面滑移。塑性变形初期位错平面滑移导致合金具有较高的初始加工硬化率[66]。位错的平面滑移并未导致材料塑性变形局域化及拉伸塑性的下降,这与传统认知相违背[67,68]。Zhang等[65]认为在合金变形后期,激发了孪晶诱导塑性变形,位错与纳米孪晶的交互作用提高了材料的加工硬化能力,从而使得材料具有较高的拉伸塑性。由于缺乏后期变形机制的研究,因此该合金的强韧化机制仍不清晰。

图4

图4   CoCrNi合金显微结构及力学性能[65]

Fig.4   Microstructure and mechanical properties of CoCrNi alloy[65]

(a, b) energy-filtered dark-field images from different diffuse superlattice peaks; examples showing the same domain contrast are marked with the arrows

(c) energy-filtered diffraction pattern of the region of interest; the red and blue circles indicate the dark-field imaging conditions of Figs.4a and b

(d) magnified view of the boxed part of the dark-field image in Fig.4a, with identified short-range-ordering (SRO) domains marked by the red circles

(e) the histogram of identified domain diameters (d is the average diameter, σ' isthe standard deviation)

(f-i) tensile mechanical properties of the CoCrNi alloys without (f, h) and with (g, i) SRO structure, respectively (DIC—digital image correlation) (Insets in Figs.4f and g are the sample images of the strain distribution during elastic leading, as determined by DIC)


最近,SRO的直接观测取得了重大的研究进展,Chen等[39]利用原子分辨元素映射技术,直观地给出了不同元素的晶格占位信息,揭示了VCoNi合金的SRO异质结构,更重要的是该研究澄清了SRO对合金变形机制及力学性能的影响。研究结果表明,VCoNi合金中的SRO尺寸为0.6 nm,体积分数约为25%,如图5a[39]所示。合金中的SRO表现为近邻V-V元素间距为近邻V-Co、V-Ni的2倍,呈现出Co(Ni)、V、Co(Ni)、V原子富集堆积顺序,如图5b[39]所示。这种短程有序结构极大提高了合金的晶格应变,从而使得位错运动缓慢,提高了位错之间的交互作用机会,导致位错缠结,从而提高材料的加工硬化率。此外,Wang等[40]在Al9.5CrCoNi高熵合金中发现了中程有序(medium-range-ordering,MRO)异质结构。相比于SRO,MRO结构具有更大的尺寸,约为2.2 nm,该结构能够稳定地存在于合金中,并不会因为位错滑移而破坏,这也使得该合金具有优异的力学性能。

图5

图5   VCoNi合金显微结构及元素分布[39]

Fig.5   Microstructure and chemical distributions of VCoNi alloy[39]

(a) HAADF-STEM image and CSRO region size distributions of VCoNi alloy (CSRO—chemical short-range order, FFT—fast Fourier transformation)

(b) atomic resolution energy dispersive spectroscopy (EDS) mapping showing the chemical distribution

(c) lattice strain (ε) distribution of VCoNi alloy before and after tensile tests, respectively (Insets in Fig.5c are a close-up view showing the edge dislocation-induced strain-field)


综上所述,SRO和MRO异质结构可以有效地改变位错运动方式,阻碍位错运动,从而提升材料的力学性能。但是由于其尺寸较小,对位错阻碍作用有限,导致材料的力学性能未能实现突破性变革。因此,该类型异构强化机制往往不会单独作用来改善合金力学性能。

2.3 纳米析出相异构

最近研究[69,70]表明,具有纳米级析出相的异构高熵合金展示出了优异的力学性能,实现了合金强度与塑性的协同提升。Yang等[34]利用L12相(γ')强化fcc结构高熵合金,设计了(FeCoNi)86Al7Ti7高熵合金。该合金通过热机械处理,呈现出L12相和fcc固溶体相双相显微结构,并且通过TEM对其显微结构表征可知,L12相的尺寸为30~50 nm,且均匀地分散在fcc基体中(图6a[34])。此外,通过原子分辨TEM像可知,L12相与fcc基体具有良好的共格关系(图6b[34]),两相的晶格错配度仅为0.21%,较低的晶格错配度使得L12相具有较高的体积分数,高达50%~55%。材料在变形过程中,与LCF和SRO异质结构一样,较高体积的L12相可以阻碍位错运动,提高位错之间交互作用,进而提高合金的强度。不同的是,相比于LCF和SRO异质结构,L12相具有较大的尺寸,可以阻碍位错穿过,从而产生的较强的Orowan强化机制[71],明显提升了合金的屈服强度。对比单相fcc结构高熵合金,纳米L12析出相异构合金屈服强度提升了4.5倍(图6c[34])。此外,该合金展示了优异的加工硬化能力,如图6d[34]所示。该合金较高的加工硬化能力有2个方面的来源:一方面,在变形初期,L12相具有较高的抵抗塑性变形的能力,导致塑性变形在fcc基体中产生,从而在异质界面处产生应变差,诱发异构变形诱导强化与硬化;另一方面,随着变形量的增加,位错密度逐渐提高,林位错整齐排列,从而形成微观变形带,产生微带诱导塑性变形。此外,微观变形带类似于小角度晶界,继续阻碍位错的运动,从而产生强化与硬化。得益于这2种强化、硬化机制,该合金实现了稳定的塑性变形,获得了较高的拉伸塑性。

图6

图6   (FeCoNi)86Al7Ti7高熵合金显微结构与室温拉伸力学性能[34]

Fig.6   Microstructure and mechanical properties of (FeCoNi)86Al7Ti7 alloy[34]

(a) TEM image

(b) high-resolution TEM image and corresponding FFT images

(c) tensile properties of (FeCoNi)86Al7Ti7 alloy at room temperature, the alloy exhibits ductile dimpled structures without macroscopic necking

(d) work-hardening rate vs true strain curves of (FeCoNi)86Al7Ti7 alloy at room temperature (MBIP—microband-induced plasticity)

(e) TEM images of the sample at different tensile strains (MBs—microbands, HDDWs—high density dislocation walls)


Liang等[72]通过调控合金化学成分,设计了高密度L12相异构Al0.5Cr0.9FeNi2.5V0.2高熵合金。通过增加Ni元素含量及添加微量V元素,促使合金发生调幅分解,从而形成了L12相与fcc基体连续分布的异质结构。图7a[72]为合金显微结构的原子分辨HAADF-STEM像,可以看出有序L12相与无序fcc基体相互交错共存,两相晶格常数与体积分数基本相同。这也意味着两相之间具有较低的晶格错配度。因此,在塑性变形过程中,位错被连续的L12相阻挡和限制,极大地提高了材料的屈服强度。此外,位错滑移切过L12与fcc相界面后会产生反向界面能,从而提高后续位错的滑移阻力,导致持续硬化,促使材料产生均匀塑性变形。这种独特的显微结构与变形机制,使得该合金具有超高的屈服强度(1800 MPa)和较高的断裂延伸率(9%)(图7b[72])。除此之外,An等[73]利用条幅分解设计理念,制备了具有纳米尺度连续异构的HfNbTiV难熔高熵合金(图7c[73]),实现了难熔高熵合金拉伸强度与塑性的协同提高(屈服强度约1100 MPa,断裂延伸率约28%) (图7c[73])。其强化机制与Al0.5Cr0.9FeNi2.5V0.2高熵合金具有相似之处,变形过程中连续的异质界面能够阻碍位错运动,提高位错运动的阻力,从而产生强化效果。不同之处在于,HfNbTiV难熔高熵合金本身具有较大的晶格畸变效果,固溶强化为合金的主要强化机制。通过计算可知,该合金固溶强化量和异质界面强化量分别为960和140 MPa。此外,该合金的高塑性得益于变形过程中异质界面对位错的阻碍作用,使得位错缓慢滑移,同时促进位错交滑移,极大地提高了位错之间的交互作用,从而提高加工硬化能力,促进材料均匀塑性变形。因此,调幅分解纳米尺度异质界面的设计为发展具有拉伸塑性的难熔高熵合金提供了新的设计思路与理论指导。

图7

图7   Al0.5Cr0.9FeNi2.5V0.2和HfNbTiV合金显微结构与拉伸力学性能[72,73]

Fig.7   Microstructures and mechanical properties of Al0.5Cr0.9FeNi2.5V0.2 andHfNbTiV alloys

(a) HAADF-STEM image and the corresponding FFT images of Al0.5Cr0.9FeNi2.5V0.2 alloy[72]

(b) tensile properties of Al0.5Cr0.9FeNi2.5V0.2 alloy at room temperature (ST—solution-treated)[72]

(c) HAADF-STEM images and the corresponding SAED patterns of HfNbTiV alloy[73]

(d) tensile property of HfNbTiV alloy at room temperature[73] (Insets are SEM images of the fracture surface)


随着纳米析出异构高熵合金的发展,Fan等[74]设计了具有层状分布的L12相异构高熵合金,极大地提高了高熵合金力学性。如图8a[74]所示,共格L12相与基体呈现出片层状交替分布的显微结构,其中L12相平均片层厚度约为30 nm,fcc基体平均片层厚度约为37 nm。这种独特的异质结构使合金获得了2026 MPa的屈服强度以及16%的均匀延伸率(图8b[74])。该合金的超高屈服强度来源于L12相对位错的阻碍作用,类似于Hall-Petch强化,较小的片层厚度(对应于较小的晶粒尺寸)使其具有较高的强化作用[75]。通过计算可知,该特殊形貌的L12相带来的强化效果高达1000 MPa。高塑性的获得主要得益于变形过程中激发的高密度层错,分布在2个{111}面的层错相互作用,形成不可动的Lomer-Cottrell位错锁(图8c[74]),从而提高了位错运动的阻力,造成硬化,促进材料均匀变形。

图8

图8   Ni32.8Fe21.9Co21.9Cr10.9Al7.5Ti5.0高熵合金显微结构与拉伸力学性能[74]

Fig.8   Microstructure and mechanical properties of Ni32.8Fe21.9Co21.9Cr10.9Al7.5Ti5.0 alloy[74]

(a) TEM image and the size distributions of L12 phase and fcc matrix

(b) tensile properties of Ni32.8Fe21.9Co21.9Cr10.9Al7.5Ti5.0 alloy at room temperature (CNL—coherent nanolamellar)

(c) TEM images of Ni32.8Fe21.9Co21.9Cr10.9Al7.5Ti5.0 alloy at different tensile strains


纳米析出相异构高熵合金并不局限于与fcc基体具有共格关系的L12析出相,还包含L21和B2相等与fcc基体具有半共格关系的析出相。Jang等[47]对Al0.2CoNiV高熵合金进行热机械处理,获得了尺寸分别为几百纳米和7.4 μm的双峰分布的L21相。并且,该L21相与fcc基体保持着Kurdjumov-Sachs (K-S)取向关系。该结构的产生源于变形过程中产生的剪切变形带,在随后的热处理过程中可以作为异质形核位点,这极大地促进了L21相的形核。这种特殊的显微结构使得该合金具有优异的强塑性匹配(屈服强度约1300 MPa,抗拉强度约1600 MPa,断裂延伸率约25%)。

综上所述,与传统析出相强化合金相比,具有纳米级析出相的异构高熵合金展示出了优异的强韧化效果,大幅提高材料屈服强度的同时还保持了合金的塑性变形能力,这使得合金具有优异的力学性能。此外,该类型异构高熵合金中析出相的三维形貌、尺寸、体积分数以及与基体的取向关系影响着合金的强塑性匹配。因此,通过合金化学成分设计以及热机械处理等手段,实现对纳米级析出相的精细调控,可以再次提升合金的力学性能。

3 微米尺度异构强韧化

3.1 晶粒异构

晶粒尺寸及分布不均匀的材料是典型的异构材料,其显微结构包括双峰结构、层状结构和梯度结构[76]。在传统金属材料中,科研人员利用晶粒异构实现了材料的强度与塑性同时提升,为高强韧异构高熵合金发展提供了参考典范[77~79]。变形后的高熵合金在退火过程中表现出相对较高的再结晶温度、较高的晶粒粗化温度和缓慢的晶粒粗化行为[80]。因此,高熵合金可以通过调控再结晶温度及热处理时间来实现对晶粒尺寸及分布的显微结构设计。Wu等[81]利用冷轧和低温热处理工艺在Al0.1CoCrFeNi高熵合金中获得了由再结晶晶粒和变形晶粒组成的异质晶粒显微结构。该合金在室温条件下具有711 MPa的屈服强度、928 MPa的抗拉强度和30.3%的均匀延伸率。相比于均匀晶粒结构合金,屈服强度提升了355 MPa的同时保持了较高的拉伸塑性。此外,利用原位SEM研究了异构合金塑性变形行为,研究表明,在塑性变形过程中,位错率先在再结晶晶粒中形核及滑移,从而在异质界面处产生应变差,诱发异构变形诱导强化与硬化,提升材料屈服强度及加工硬化能力。随着变形的增加,位错在变形晶粒中产生与滑移。该实验采用了循环加载-卸载拉伸方法,定量化分析了异构诱导塑性变形强化量,研究结果显示该异构合金在屈服点的异构变形诱导强化量高达约400 MPa。

Zhang等[44]对Nb55Ta25Ti15Hf5难熔合金进行冷轧和低温热处理,获得了由细晶和粗晶组成的层状分布异构晶粒组织,该组织在室温下的屈服强度约为620 MPa,同时均匀延伸率可以达到约6%。在拉伸变形过程中,相邻的不同尺寸晶粒之间存在较大的应变差,从而产生异构变形诱导强化与硬化效应,这使得合金在一定应变范围内保持了高的加工硬化效果。

异构晶粒的获得不止局限于热机械处理手段,样品表面处理工艺同样可以实现不同尺寸的晶粒在空间范围内分布的调控,从而获得具有梯度分布的异构晶粒。样品表面处理工艺包括旋转加速喷丸技术(RASP)、表面机械研磨处理工艺(surface mechanical attrition treatment,SMAT)和循环扭转工艺[41,82,83]。其中利用RASP技术可以在低层错能高熵合金中实现不同梯度层次的异质结构,包括孪晶密度梯度、位错密度梯度以及分层纳米孪晶梯度。Hasan等[84]对等摩尔CoCrFeNiMn高熵合金进行RASP处理,获得了由梯度晶粒组成的异构组织(图9a~c[84])。相较于均匀晶粒组织,该梯度组织使得合金屈服强度提高了95 MPa。同时,梯度组织合金的拉伸塑性并未下降。这是由于在拉伸变形过程中,梯度晶粒结构促使形成梯度的应变分布,诱导产生高密度的几何必需位错(图9d~g[84]),从而产生较大的异构变形诱导硬化,提高合金强度的同时保持了合金塑性。

图9

图9   CoCrFeNiMn高熵合金拉伸变形前后显微结构特征[84]

Fig.9   Microstructures of RASP CoCrFeNiMn alloy before and after tensile tests[84] (RASP—rotationally accelerated shot peening, CG—coarse grain, TD—tensile direction, LD—longitudinal direction)

(a) typical IPF image before tensile test (IPF—inverse pole figure)

(b) image quality map before tensile test

(c) KAM map before tensile test (KAM—kernel average misorientation)

(d) image quality map of the coarse grain sample after tensile test

(e) KAM map of the coarse grain sample after tensile test

(f) image quality map of the RASP sample after tensile tests

(g) KAM map of the RASP sample after tensile test


上述研究结果表明,与常规均匀晶粒结构相比,异质晶粒显微结构高熵合金具有更高强度的同时能够保持合金的拉伸塑性。同时,该显微结构设计还能够提高难熔高熵合金拉伸强度与塑性。异构晶粒组织提高合金力学性能的优势在于变形过程中诱发异构变形诱导强化与硬化效应,大幅提高合金加工硬化能力,从而实现提升强度的同时保持较高的拉伸塑性。

3.2 双相异构

共晶高熵合金(eutectic high-entropy alloy,EHEA)作为一种典型的双相异构材料,展示出了良好的强度-塑性匹配[85~88]。Lu等[89]利用“共晶”设计理念首次设计出了AlCoCrFeNi2.1共晶高熵合金。该铸态合金呈现出B2相与fcc相交替存在的微观结构,从而形成连续双相的异质结构。力学性能测试结果表明,该合金具有优异的力学性能:抗拉强度高达944 MPa,断裂延伸率为22.8%。随着共晶高熵合金发展,Shi等[85]设计了Fe20Co20Ni41Al19共晶高熵合金,获得了B2相和fcc相层状分布的异构显微结构,其中fcc相片层厚度约为1.85 μm,B2相片层厚度约为0.46 μm。这种特殊的显微结构使得该合金呈现出较高的屈服强度(1220 MPa)及断裂延伸率(24%)。在变形过程中,较软的fcc相率先发生塑性变形,使得B2与fcc相异质界面处产生几何必需位错,从而产生背应力强化,使得该合金表现出较高的屈服强度。此外,几何必需位错堆积造成B2相产生前应力,促进B2相发生塑性变形。因此,在B2相与fcc相之间存在应变梯度,从而激发异构变形诱导硬化,提高材料加工硬化能力。随着变形的增加,fcc相发生孪晶诱导塑性变形,再次提高材料加工硬化能力,从而实现较大的拉伸塑性。最近,该课题组利用定向凝固技术制备了“鱼骨状”Fe20Co20Ni41Al19异构高熵合金,获得了类似鱼骨状分布的L12/B2双相异质结构[35],如图10[35]所示。变形过程中,异质界面能够有效地阻碍位错运动,产生异构变形诱导强化及硬化。随着变形的增加,裂纹在B2相中产生并扩展,当遇到L12相时,裂纹被阻挡而终止。因此,该异质结构可以有效地阻挡裂纹扩展,增加材料损伤容限,使得该合金具有670 MPa的屈服强度与50%的均匀延伸率[35]。

图10

图10   Fe20Co20Ni41Al19高熵合金鱼骨状显微结构[35]

Fig.10   Hierarchically arranged herringbone microstructure of Fe20Co20Ni41Al19 high entropy alloy[35]

(a-c) conventionally cast eutectic high-entropy alloy (EHEA) serving here as reference material

(a) SEM backscattered electron image

(b) electron backscattering diffraction (EBSD) phase map (left) and IPF map (right)

(c) schematic diagram

(d-i) directionally solidified EHEA with a hierarchical herringbone microstructure (The black arrows in Figs.10d and e indicate the directional solidification (DS) direction; AEC—aligned eutectic colonies, BEC—branched eutectic colonies)

(d) SEM backscatter electron image showing that the microstructure is composed of columnar grains. Grain boundaries are marked by black dashed lines

(e) enlarged EBSD phase and IPF maps showing the columnar grain consisting of AEC and BEC. Black solid and dashed lines mark grain and colony boundaries, respectively

(f, i) schematic diagram of herringbone structure and its formation principle, respectively

(g) HAADF-STEM image and related SAED patterns of B2 and L12 phases. The HAADF-STEM image shows clean dual-phase lamellae without evidence of nanoprecipitates or other phases, as is also indicated in Fig.10f

(h) synchrotron high-energy X-ray diffraction (SHE-XRD) of B2 and L12 phases


上述研究表明,与传统单相合金相比,设计具有双相共晶异构显微结构可以实现材料加工硬化率的显著提升,这是由于变形过程中异质界面产生梯度应变从而激发几何必需位错的产生,诱发异构变形诱导强化与硬化。此外,双相结构可以阻碍裂纹扩展,提高材料损伤容限。结合上述2种优势,双相异构高熵合金实现了材料强度与塑性的同时提高。

4 跨纳米-微米尺度多级异构强韧化

高熵合金通过化学成分设计及热机械处理等方式可以实现纳米、微米尺度异构显微结构。与单相均匀结构高熵合金相比,具有异构组织的高熵合金实现了强度与塑性的同时提高,获得了高强韧的力学性能。而在纳米尺度异构基础之上,引入微米尺度异构结构,获得跨纳米-微米尺度异构组织,可以进一步提升合金的强塑性匹配。因此,深入分析跨尺度异构结构对合金强韧化和力学性能的影响机制,对设计异构高熵合金组织及发展高强韧高熵合金材料具有重要意义。

4.1 跨尺度晶粒异构

Yang等[46]利用冷轧和低温再结晶处理获得了由纳米晶、超细晶和粗晶组成的跨纳米-微米尺度晶粒异构CoCrNi合金。其中纳米晶、超细晶以及粗晶晶粒尺寸分别为250 nm、250 nm~1 μm和2.3 μm,体积分数分别为43%、47%和10%。此外,纳米晶大多分布在晶界处,而超细晶分布在三叉晶界处(图11a[46])。这种特殊的显微组织使得该合金表现出优异的屈服强度,室温屈服强度高达1150 MPa。在室温拉伸变形过程中,异构晶粒之间的应变分配使得该合金表现出较强的异构变形诱导强化与硬化(图11b[46])。由于合金具有较高的强度,随着变形量增加,产生孪晶诱导塑性变形,晶界处不断形成纳米孪晶,使合金获得进一步动态强化(图11c[46])。同时,晶粒内部也开始激活层错、孪晶等塑性变形机制,使得材料加工硬化率再次提升。得益于高的加工硬化能力,合金展示出了较高的拉伸塑性,均匀延伸率为22%。

图11

图11   CoCrNi合金晶粒异构显微结构及异构结构中的异构变形诱导硬化[46]

Fig.11   Microstructure and hetero-deformation induced (HDI) hardening of CoCrNi alloy[46]

(a) EBSD and TEM image of CoCrNi alloy (LAGB—low angle grain boundary, HAGB—high-angle grain boundary, TB—twin boundary, UFG—ultrafine-grained)

(b) true stress-strain curves during LUR (loading-unloading-reloading) tests at 298 K and 77 K. Hysteresis loops at the maximum uniform strain. Comparison of HDI hardening with the total strain hardening in the CoCrNi alloy at 298 K and 77 K (εrp—reverse plastic strain, σf—flow stress, σ0.2—yield stress, σb—back stress, σb, 0.2—back stress at yielding)

(c) TEM image of the deformed CoCrNi alloy (NG—nanograin)


除此之外,An等[42]利用RASP技术在新型非等摩尔Co21.5Cr21.5Fe21.5Mn21.5Ni14高熵合金中引入了梯度纳米孪晶和梯度微米晶粒异构显微组织:由样品表面到中心内部,纳米孪晶的片层厚度逐渐增加(由约7 nm增加到70 nm),晶粒尺寸逐渐增加(由约9 μm增加到25 μm),如图12[42]所示。在变形初期,样品表面细晶区产生孪晶诱导塑性变形,形成多级纳米孪晶结构;而在样品内部粗晶区,仅由位错运动主导材料塑性变形。因此,梯度晶粒之间存在较大的应变差异,从而在异质晶粒界面处产生应变梯度,引起异构变形诱导硬化,提高材料加工硬化率。此外,随着变形的增加,材料流动应力不断增加,表面细晶粒内部开始产生微观变形带诱导塑性变形。同时,粗晶粒内部激发多种变形方式,例如,位错、层错和孪晶,从而进一步提高材料加工硬化能力。结合这2种强韧化方式,跨纳米-微米尺度异构晶粒组织获得了较高拉伸屈服强度(750 MPa)和塑性(27.5%)的匹配。相比均匀晶粒分布的高熵合金,其屈服强度提升了275%,同时保持了合金的拉伸塑性。

图12

图12   Co21.5Cr21.5Fe21.5Mn21.5Ni14高熵合金经过RASP处理后的梯度组织[42]

Fig.12   Gradient microstructures of the RASP treated Co21.5Cr21.5Fe21.5Mn21.5Ni14 alloy[42]

(a) schematic of the grain size gradient through the plate thickness

(b-d) EBSD images of the alloy at different depths from the surface

(e-g) TEM images of twin structures in regions (I), (II) and (III) (The insets are SAED patterns from each region)

(h) a high-resolution HAADF-STEM image of the deformation twins in region (I)

(i) variation of the average grain size through the plate thickness

(j) variation of the average thickness of deformation twins through the plate thickness


综上所述,在单一尺度晶粒异构的基础之上,通过显微组织调控,获得具有跨尺度异构的晶粒结构可以实现高熵合金力学性能的再次提高。这归因于跨尺度异构组织可以充分利用异构变形诱导硬化机制,提升材料加工硬化能力,同时,跨尺度异构材料的高强度使得合金诱发其他变形机制,例如,层错和孪晶,从而再次提升材料加工硬化能力。最终,跨尺度晶粒异构材料实现了高强度与高塑性的完美结合。

4.2 跨尺度析出相异构

如前文所述,相比于单相fcc结构高熵合金,纳米级析出相异构高熵合金可以实现材料强度的大幅提高。而在纳米级析出相基础之上,引入跨尺度多级析出相异构显微组织,可以使材料的力学性能获得进一步提升。鉴于此,Fu等[90]设计了Fe25Co25Ni25Al10Ti15高熵合金,并通过热机械处理,获得了由微米级bcc相(0.3 μm)、纳米级L12相(约57 nm)和二次L12相(约10 nm)组成的多级析出相异构组织,该组织室温下拉伸屈服强度高达1860 MPa,断裂强度高达2520 MPa,同时具有5.2%的均匀延伸率。在拉伸变形过程中,多级析出相结构能够有效地阻碍位错运动,从而极大地提升合金强度。同时,在fcc基体中产生孪晶、层错等变形机制,提升了合金的加工硬化能力。此外,相邻的异质相结构之间存在较大背应力,产生异构变形诱导硬化,使得合金加工硬化率再次提升,从而获得了较高的均匀延伸率。

相似的,Jia等[91]设计了新型Ni46Co24Fe24Al3Ti3高熵合金,该铸态fcc结构高熵合金晶粒内部由立方形貌和球形形貌2种L12析出相组成,从而形成了一种多相异构组织。该铸态合金展示了优异的拉伸力学性能:屈服强度525 MPa,抗拉强度935 MPa,断裂延伸率32%,相比于单相铸态fcc结构高熵合金,屈服强度提高了约350 MPa。

因此,这些工作证明了在纳米级析出相异构高熵合金基础上引入跨尺度多级析出相异构可以进一步提升材料的力学性能。

4.3 跨尺度晶粒、析出相双重异构

上述研究表明,相比于单一尺度异构材料,跨尺度晶粒、析出相异构材料展示出了更好的强韧化效果。因此可以推测,将单一晶粒、析出相异构组织进行耦合,设计具有跨尺度晶粒-析出相双重异构显微组织的材料将实现力学性能的巨大突破。

Du等[48]对Co34.46Cr32.12Ni27.42Al3Ti3高熵合金进行深冷轧制与再结晶处理,获得由粗晶(10~30 μm)和纳米晶(500 nm~2 μm)组成的跨尺度晶粒异构的显微组织。同时,在晶粒内部及晶界处形成了尺寸分别为约100 nm和20~50 nm的多级L12析出相。因此,该合金实现了跨尺度晶粒、析出相双重异构显微组织,该组织在室温下的屈服强度高达1500 MPa,同时均匀延伸率可以达到25%。此外,对该合金进行低温时效处理,结果发现晶粒尺寸并没有变化,并且在fcc晶粒内部形成了高密度、更小尺寸的L12 析出相(约5 nm)以及退火孪晶,再次提高了合金的力学性能,该组织在室温下的屈服强度高达2000 MPa。得益于合金变形过程中产生的高密度层错及孪晶,该合金获得了较高的加工硬化能力,从而实现了较大的均匀延伸率(约13%)。

相似的,Qin等[92]对Al0.5Cr0.9FeNi2.5V0.2高熵合金进行SMAT和热机械处理,获得了由梯度晶粒和纳米析出相组成的跨尺度双重异构组织,该组织室温下屈服强度高达960 MPa,均匀延伸率约为16% (图13a[92])。相比于均匀粗晶合金,屈服强度提高了620 MPa。更重要的是,材料的加工硬化率得到了明显提升,如图13b[92]所示。在变形过程中,梯度晶粒、析出相结构产生了严重的应变梯度,从而诱发高密度几何必需位错,产生较大的异构变形诱导硬化。此外,由于B2相和L12相对位错的阻碍作用,使得位错在相界面处积累,提高了位错密度,产生析出相、位错强化与硬化机制。这3种强化与硬化机制使得该合金产生了较大的加工硬化能力。

图13

图13   粗晶、表面机械研磨处理(SMAT)和SMAT +时效处理样品拉伸力学性能[92]

Fig.13   Tensile properties for coarse grain (CG), SMAT and SMAT-aged samples[92] (SMAT—surface mechanical attrition treatment)

(a) engineering stress-strain curves

(b) hardening rate and true stress as a function of true strain


综上可以看出,将晶粒尺寸异构与纳米析出相异构进行耦合,可以产生更好的强化效果,这得益于材料在变形过程中产生了更加明显的异构变形诱导强化与硬化效果。此外,耦合析出相强化与硬化机制以及位错强化机制使得跨尺度双重异构材料能够获得高强度与高塑性的力学性能。

5 总结及展望

高熵合金自2004年被提出至今,经历了快速发展,与传统金属材料相比,其具有两大优势:一方面是巨大的化学成分调控空间,使其能够产生成百上千万种成分组合;另一方面是潜在的优异力学性能,能够填补传统金属材料力学性能的不足,解决我国重大领域中高强韧金属材料的需求。然而,金属材料的力学性能与其显微结构密不可分。因此设计和开发新型显微结构是获得优异力学性能的关键。通过对传统金属材料强韧化方法研究发现,异构显微结构设计是获得高强韧金属材料最有效的手段。因此,异构高熵合金显微组织设计与开发成为了当下高熵合金强韧化研究的重点与热点。

高熵合金的化学成分设计空间为其显微结构调控提供了无限可能。首先,高浓度的多主元元素混乱分布使得高熵合金呈现出成分波动和中/短程有序纳米尺度异构。这种纳米尺度异构可以明显提高材料屈服强度与塑性。同时该异构组织的探索与实验表征也取得了巨大进步。此外,研究者通过在单相CoCrFeNi基高熵合金中添加个别元素,例如,Al、Ti等,获得了具有纳米析出相异构的高熵合金。这种纳米析出相异构显微组织可以大幅提高材料屈服强度,同时获得较高的加工硬化能力,促进材料均匀塑性变形,实现材料强度-塑性的匹配。其次,通过材料加工工艺的调控,将均匀晶粒调整为异构晶粒,实现了高熵合金材料跨纳米、微米尺度异构。这种多级异构高熵合金充分利用了异构变形诱导强化与硬化机制,大幅提高了材料加工硬化能力,实现了材料力学性能的再次突破。最后,通过化学元素以及加工工艺调控,可获得具有跨纳米、微米尺度晶粒、析出相双重异构高熵合金材料。该异构材料可以耦合多种强化硬化机制,实现材料超高强度与塑性的完美结合。

因此,在后续的研究中,通过合金化学成分设计、合金加工工艺调控,实现对高熵合金中析出相尺寸、三维形貌、体积分数调控以及晶粒尺寸、分布精细调控,获得具有跨尺度晶粒、析出相等多级异构高熵合金,是实现高熵合金力学性能再次突破的关键手段。然而,如何更好构筑多种异构显微结构单元,使多种强韧化机制获得充分发挥,从而进一步改善合金力学性能,仍是未来研究的重点与难点。

参考文献

Zherebtsov S, Salishchev G, Galeyev R, et al.

Mechanical properties of Ti-6Al-4V titanium alloy with submicrocrystalline structure produced by severe plastic deformation

[J]. Mater. Trans., 2005, 46: 2020

DOI      URL     [本文引用: 1]

Chong Y, Zhang R P, Hooshmand M S, et al.

Elimination of oxygen sensitivity in α-titanium by substitutional alloying with Al

[J]. Nat. Commun., 2021, 12: 6158

DOI      PMID      [本文引用: 1]

Individually, increasing the concentration of either oxygen or aluminum has a deleterious effect on the ductility of titanium alloys. For example, extremely small amounts of interstitial oxygen can severely deteriorate the tensile ductility of titanium, particularly at cryogenic temperatures. Likewise, substitutional aluminum will decrease the ductility of titanium at low-oxygen concentrations. Here, we demonstrate that, counter-intuitively, significant additions of both Al and O substantially improves both strength and ductility, with a 6-fold increase in ductility for a Ti-6Al-0.3 O alloy as compared to a Ti-0.3 O alloy. The Al and O solutes act together to increase and sustain a high strain-hardening rate by modifying the planar slip that predominates into a delocalized, three-dimensional dislocation pattern. The mechanism can be attributed to decreasing stacking fault energy by Al, modification of the "shuffle" mechanism of oxygen-dislocation interaction by the repulsive Al-O interaction in Ti, and micro-segregation of Al and O by the same cause.© 2021. This is a U.S. Government work and not under copyright protection in the US; foreign copyright protection may apply.

Huskins E L, Cao B, Ramesh K T.

Strengthening mechanisms in an Al-Mg alloy

[J]. Mater. Sci. Eng., 2010, A527: 1292

[本文引用: 1]

Altıparmak S C, Yardley V A, Shi Z S, et al.

Challenges in additive manufacturing of high-strength aluminium alloys and current developments in hybrid additive manufacturing

[J]. Int. J. Lightweight Mater. Manuf., 2021, 4: 246

[本文引用: 1]

Wei Y J, Li Y Q, Zhu L C, et al.

Evading the strength-ductility trade-off dilemma in steel through gradient hierarchical nanotwins

[J]. Nat. Commun., 2014, 5: 3580

DOI      PMID      [本文引用: 1]

The strength-ductility trade-off has been a long-standing dilemma in materials science. This has limited the potential of many structural materials, steels in particular. Here we report a way of enhancing the strength of twinning-induced plasticity steel at no ductility trade-off. After applying torsion to cylindrical twinning-induced plasticity steel samples to generate a gradient nanotwinned structure along the radial direction, we find that the yielding strength of the material can be doubled at no reduction in ductility. It is shown that this evasion of strength-ductility trade-off is due to the formation of a gradient hierarchical nanotwinned structure during pre-torsion and subsequent tensile deformation. A series of finite element simulations based on crystal plasticity are performed to understand why the gradient twin structure can cause strengthening and ductility retention, and how sequential torsion and tension lead to the observed hierarchical nanotwinned structure through activation of different twinning systems.

Yeh J W, Chen S K, Lin S J, et al.

Nanostructured high-entropy alloys with multiple principal elements: Novel alloy design concepts and outcomes

[J]. Adv. Eng. Mater., 2004, 6: 299

DOI      URL     [本文引用: 1]

Cantor B, Chang I T H, Knight P, et al.

Microstructural development in equiatomic multicomponent alloys

[J]. Mater. Sci. Eng., 2004, A375-377: 213

[本文引用: 1]

Yeh J W.

Recent progress in high-entropy alloys

[J]. Ann. Chim. Sci. Mat., 2006, 31: 633

DOI      URL     [本文引用: 2]

Zhang W R, Liaw P K, Zhang Y.

Science and technology in high-entropy alloys

[J]. Sci. China Mater., 2018, 61: 2

DOI      URL     [本文引用: 1]

George E P, Raabe D, Ritchie R O.

High-entropy alloys

[J]. Nat. Rev. Mater., 2019, 4: 515

DOI      [本文引用: 1]

Alloying has long been used to confer desirable properties to materials. Typically, it involves the addition of relatively small amounts of secondary elements to a primary element. For the past decade and a half, however, a new alloying strategy that involves the combination of multiple principal elements in high concentrations to create new materials called high-entropy alloys has been in vogue. The multi-dimensional compositional space that can be tackled with this approach is practically limitless, and only tiny regions have been investigated so far. Nevertheless, a few high-entropy alloys have already been shown to possess exceptional properties, exceeding those of conventional alloys, and other outstanding high-entropy alloys are likely to be discovered in the future. Here, we review recent progress in understanding the salient features of high-entropy alloys. Model alloys whose behaviour has been carefully investigated are highlighted and their fundamental properties and underlying elementary mechanisms discussed. We also address the vast compositional space that remains to be explored and outline fruitful ways to identify regions within this space where high-entropy alloys with potentially interesting properties may be lurking.

Gludovatz B, Hohenwarter A, Catoor D, et al.

A fracture-resistant high-entropy alloy for cryogenic applications

[J]. Science, 2014, 345: 1153

DOI      PMID      [本文引用: 1]

High-entropy alloys are equiatomic, multi-element systems that can crystallize as a single phase, despite containing multiple elements with different crystal structures. A rationale for this is that the configurational entropy contribution to the total free energy in alloys with five or more major elements may stabilize the solid-solution state relative to multiphase microstructures. We examined a five-element high-entropy alloy, CrMnFeCoNi, which forms a single-phase face-centered cubic solid solution, and found it to have exceptional damage tolerance with tensile strengths above 1 GPa and fracture toughness values exceeding 200 MPa·m(1/2). Furthermore, its mechanical properties actually improve at cryogenic temperatures; we attribute this to a transition from planar-slip dislocation activity at room temperature to deformation by mechanical nanotwinning with decreasing temperature, which results in continuous steady strain hardening. Copyright © 2014, American Association for the Advancement of Science.

Schuh B, Mendez-Martin F, Völker B, et al.

Mechanical properties, microstructure and thermal stability of a nanocrystalline CoCrFeMnNi high-entropy alloy after severe plastic deformation

[J]. Acta Mater., 2015, 96: 258

DOI      URL     [本文引用: 1]

Ding Z Y, Cao B X, Luan J H, et al.

Synergistic effects of Al and Ti on the oxidation behaviour and mechanical properties of L12-strengthened FeCoCrNi high-entropy alloys

[J]. Corros. Sci., 2021, 184: 109365

DOI      URL     [本文引用: 1]

Geng Y S, Chen J, Tan H, et al.

Vacuum tribological behaviors of CoCrFeNi high entropy alloy at elevated temperatures

[J]. Wear, 2020, 456-457: 203368

DOI      URL     [本文引用: 1]

Zhang Y, Zhou Y J, Lin J P, et al.

Solid-solution phase formation rules for multi-component alloys

[J]. Adv. Eng. Mater., 2008, 10: 534

DOI      URL     [本文引用: 1]

Guo S, Ng C, Lu J, et al.

Effect of valence electron concentration on stability of fcc or bcc phase in high entropy alloys

[J]. J. Appl. Phys., 2011, 109: 103505

DOI      URL    

Oh H S, Kim S J, Odbadrakh K, et al.

Engineering atomic-level complexity in high-entropy and complex concentrated alloys

[J]. Nat. Commun., 2019, 10: 2090

DOI      PMID      [本文引用: 1]

Quantitative and well-targeted design of modern alloys is extremely challenging due to their immense compositional space. When considering only 50 elements for compositional blending the number of possible alloys is practically infinite, as is the associated unexplored property realm. In this paper, we present a simple property-targeted quantitative design approach for atomic-level complexity in complex concentrated and high-entropy alloys, based on quantum-mechanically derived atomic-level pressure approximation. It allows identification of the best suited element mix for high solid-solution strengthening using the simple electronegativity difference among the constituent elements. This approach can be used for designing alloys with customized properties, such as a simple binary NiV solid solution whose yield strength exceeds that of the Cantor high-entropy alloy by nearly a factor of two. This study provides general design rules that enable effective utilization of atomic level information to reduce the immense degrees of freedom in compositional space without sacrificing physics-related plausibility.

Zhou Z Q, Zhou Y J, He Q F, et al.

Machine learning guided appraisal and exploration of phase design for high entropy alloys

[J]. npj Comput. Mater., 2019, 5: 128

DOI      URL    

Wang Z J, Huang Y H, Yang Y, et al.

Atomic-size effect and solid solubility of multicomponent alloys

[J]. Scr. Mater., 2015, 94: 28

DOI      URL     [本文引用: 1]

Senkov O N, Scott J M, Senkova S V, et al.

Microstructure and room temperature properties of a high-entropy TaNbHfZrTi alloy

[J]. J. Alloys Compd., 2011, 509: 6043

DOI      URL     [本文引用: 1]

Senkov O N, Wilks G B, Scott J M, et al.

Mechanical properties of Nb25Mo25Ta25W25 and V20Nb20Mo20Ta20W20 refractory high entropy alloys

[J]. Intermetallics, 2011, 19: 698

DOI      URL     [本文引用: 1]

Huang H L, Wu Y, He J Y, et al.

Phase-transformation ductilization of brittle high-entropy alloys via metastability engineering

[J]. Adv. Mater., 2017, 29: 1701678

DOI      URL     [本文引用: 1]

Wu Z, Bei H, Pharr G M, et al.

Temperature dependence of the mechanical properties of equiatomic solid solution alloys with face-centered cubic crystal structures

[J]. Acta Mater., 2014, 81: 428

DOI      URL     [本文引用: 1]

Rao J C, Diao H Y, Ocelík V, et al.

Secondary phases in Al x CoCrFeNi high-entropy alloys: An in-situ TEM heating study and thermodynamic appraisal

[J]. Acta Mater., 2017, 131: 206

DOI      URL     [本文引用: 1]

Park J M, Yang D C, Kim H J, et al.

Ultra-strong and strain-hardenable ultrafine-grained medium-entropy alloy via enhanced grain-boundary strengthening

[J]. Mater. Res. Lett., 2021, 9: 315

DOI      URL     [本文引用: 4]

Gwalani B, Soni V, Lee M, et al.

Optimizing the coupled effects of Hall-Petch and precipitation strengthening in a Al0.3CoCrFeNi high entropy alloy

[J]. Mater. Des., 2017, 121: 254

DOI      URL    

He Y X, Yang H X, Zhao C D, et al.

Enhancing mechanical properties of Al0.25CoCrFeNi high-entropy alloy via cold rolling and subsequent annealing

[J]. J. Alloys Compd., 2020, 830: 154645

DOI      URL     [本文引用: 1]

He F, Chen D, Han B, et al.

Design of D022 superlattice with superior strengthening effect in high entropy alloys

[J]. Acta Mater., 2019, 167: 275

DOI      URL     [本文引用: 1]

Chen D, He F, Han B, et al.

Synergistic effect of Ti and Al on L12-phase design in CoCrFeNi-based high entropy alloys

[J]. Intermetallics, 2019, 110: 106476

DOI      URL    

Liu W H, Lu Z P, He J Y, et al.

Ductile CoCrFeNiMox high entropy alloys strengthened by hard intermetallic phases

[J]. Acta Mater., 2016, 116: 332

DOI      URL     [本文引用: 1]

Naeem M, He H Y, Harjo S, et al.

Extremely high dislocation density and deformation pathway of CrMnFeCoNi high entropy alloy at ultralow temperature

[J]. Scr. Mater., 2020, 188: 21

DOI      URL     [本文引用: 1]

Deng Y, Tasan C C, Pradeep K G, et al.

Design of a twinning-induced plasticity high entropy alloy

[J]. Acta Mater., 2015, 94: 124

DOI      URL     [本文引用: 1]

Li Z M, Pradeep K G, Deng Y, et al.

Metastable high-entropy dual-phase alloys overcome the strength-ductility trade-off

[J]. Nature, 2016, 534: 227

DOI      URL     [本文引用: 1]

Yang T, Zhao Y L, Tong Y, et al.

Multicomponent intermetallic nanoparticles and superb mechanical behaviors of complex alloys

[J]. Science, 2018, 362: 933

DOI      PMID      [本文引用: 12]

Alloy design based on single-principal-element systems has approached its limit for performance enhancements. A substantial increase in strength up to gigapascal levels typically causes the premature failure of materials with reduced ductility. Here, we report a strategy to break this trade-off by controllably introducing high-density ductile multicomponent intermetallic nanoparticles (MCINPs) in complex alloy systems. Distinct from the intermetallic-induced embrittlement under conventional wisdom, such MCINP-strengthened alloys exhibit superior strengths of 1.5 gigapascals and ductility as high as 50% in tension at ambient temperature. The plastic instability, a major concern for high-strength materials, can be completely eliminated by generating a distinctive multistage work-hardening behavior, resulting from pronounced dislocation activities and deformation-induced microbands. This MCINP strategy offers a paradigm to develop next-generation materials for structural applications.Copyright © 2018 The Authors, some rights reserved; exclusive licensee American Association for the Advancement of Science. No claim to original U.S. Government Works.

Shi P J, Li R G, Li Y, et al.

Hierarchical crack buffering triples ductility in eutectic herringbone high-entropy alloys

[J]. Science, 2021, 373: 912

DOI      PMID      [本文引用: 6]

In human-made malleable materials, microdamage such as cracking usually limits material lifetime. Some biological composites, such as bone, have hierarchical microstructures that tolerate cracks but cannot withstand high elongation. We demonstrate a directionally solidified eutectic high-entropy alloy (EHEA) that successfully reconciles crack tolerance and high elongation. The solidified alloy has a hierarchically organized herringbone structure that enables bionic-inspired hierarchical crack buffering. This effect guides stable, persistent crystallographic nucleation and growth of multiple microcracks in abundant poor-deformability microstructures. Hierarchical buffering by adjacent dynamic strain-hardened features helps the cracks to avoid catastrophic growth and percolation. Our self-buffering herringbone material yields an ultrahigh uniform tensile elongation (~50%), three times that of conventional nonbuffering EHEAs, without sacrificing strength.Copyright © 2021 The Authors, some rights reserved; exclusive licensee American Association for the Advancement of Science. No claim to original U.S. Government Works.

Wei D X, Li X Q, Schönecker S, et al.

Development of strong and ductile metastable face-centered cubic single-phase high-entropy alloys

[J]. Acta Mater., 2019, 181: 318

DOI      URL     [本文引用: 1]

Ma E, Wu X L.

Tailoring heterogeneities in high-entropy alloys to promote strength-ductility synergy

[J]. Nat. Commun., 2019, 10: 5623

DOI      PMID      [本文引用: 2]

Conventional alloys are usually based on a single host metal. Recent high-entropy alloys (HEAs), in contrast, employ multiple principal elements. The strength of HEAs is considerably higher than traditional solid solutions, as the many constituents lead to a rugged energy landscape that increases the resistance to dislocation motion, which can also be retarded by other heterogeneities. The wide variety of nanostructured heterogeneities in HEAs, including those generated on the fly during tensile straining, also offer elevated strain-hardening capability that promotes uniform tensile ductility. Citing recent examples, this review explores the multiple levels of heterogeneities in multi-principal-element alloys that contribute to lattice friction and back stress hardening, as a general strategy towards strength-ductility synergy beyond current benchmark ranges.

Ding Q Q, Zhang Y, Chen X, et al.

Tuning element distribution, structure and properties by composition in high-entropy alloys

[J]. Nature, 2019, 574: 223

DOI      URL     [本文引用: 10]

Chen X F, Wang Q, Cheng Z Y, et al.

Direct observation of chemical short-range order in a medium-entropy alloy

[J]. Nature, 2021, 592: 712

DOI      URL     [本文引用: 6]

Wang J, Jiang P, Yuan F P, et al.

Chemical medium-range order in a medium-entropy alloy

[J]. Nat. Commun., 2022, 13: 1021

DOI      PMID      [本文引用: 2]

High-/medium-entropy alloys (H/MEA) have the inherent local chemical order. Yet, as a structural link between the incipient short-range order and mature long-range counterpart, the chemical medium-range order (CMRO) is conjectural and remains open questions as to if, and what kind of, CMRO would be produced and if CMRO is mechanically stable during plastic deformation. Here, we show compelling evidences for CMRO in an AlCrCoNi MEA. Specifically, the electron diffraction under both [[Formula: see text]] and [[Formula: see text]] zone axis show the definite spots for CMRO of lattice periodicity. CMRO entities are seen directly of medium-ranged in sizes by using dark-field imaging, along with the tendency towards like-pair avoidance and unlike-pair preference based on atomic-resolution EDS mapping. These findings substantiate CMRO with a realistic structural picture in view of crystal periodicity and chemical species occupation, shedding light on understanding the microstructural link at an extended length scale beyond the short-range order.© 2022. The Author(s).

Pan Q S, Zhang L X, Feng R, et al.

Gradient cell-structured high-entropy alloy with exceptional strength and ductility

[J]. Science, 2021, 374: 984

DOI      URL     [本文引用: 2]

An Z B, Mao S C, Liu Y N, et al.

Hierarchical grain size and nanotwin gradient microstructure for improved mechanical properties of a non-equiatomic CoCrFeMnNi high-entropy alloy

[J]. J. Mater. Sci. Technol., 2021, 92: 195

DOI      [本文引用: 5]

This study explored a multi-mechanism approach to improving the mechanical properties of a CoCrFeMnNi high-entropy alloy through non-equiatomic alloy design and processing. The alloy design ensures a single-phase face-centered cubic structure while lowering the stacking fault energy to encourage the formation of deformation twins and stacking faults by altering the equiatomic composition of the alloy. The processing strategy applied helped create a hierarchical grain size gradient microstructure with a high nanotwins population. This was achieved by means of rotationally accelerated shot peening (RASP). The non-equiatomic CoCrFeMnNi high-entropy alloy achieved a yield strength of 750 MPa, a tensile strength of 1050 MPa, and tensile uniform elongation of 27.5%. The toughness of the alloy was 2.53 × 1010 kJ/m3, which is about 2 times that of the same alloy without the RASP treatment. The strength increase is attributed to the effects of grain boundary strengthening, dislocation strengthening, twin strengthening, and hetero-deformation strengthening associated with the heterogeneous microstructure of the alloy. The concurrent occurrence of the multiple deformation mechanisms, i.e., dislocation deformation, twining deformation and microband deformation, contributes to achieving a suitable strain hardening of the alloy that helps to prevent early necking and to assure steady plastic deformation for high toughness.

Zheng X Y, Xie W B, Zeng L F, et al.

Achieving high strength and ductility in a heterogeneous-grain-structured CrCoNi alloy processed by cryorolling and subsequent short-annealing

[J]. Mater. Sci. Eng., 2021, A821: 141610

[本文引用: 4]

Zhang C, MacDonald B E, Guo F W, et al.

Cold-workable refractory complex concentrated alloys with tunable microstructure and good room-temperature tensile behavior

[J]. Scr. Mater., 2020, 188: 16

DOI      URL     [本文引用: 2]

Zhu Y T, Wu X L.

Perspective on hetero-deformation induced (HDI) hardening and back stress

[J]. Mater. Res. Lett., 2019, 7: 393

DOI      URL     [本文引用: 2]

Yang M X, Yan D S, Yuan F P, et al.

Dynamically reinforced heterogeneous grain structure prolongs ductility in a medium-entropy alloy with gigapascal yield strength

[J]. Proc. Natl. Acad. Sci. USA, 2018, 115: 7224

DOI      URL     [本文引用: 9]

Jang T J, Choi W S, Kim D W, et al.

Shear band-driven precipitate dispersion for ultrastrong ductile medium-entropy alloys

[J]. Nat. Commun., 2021, 12: 4703

DOI      PMID      [本文引用: 1]

Precipitation strengthening has been the basis of physical metallurgy since more than 100 years owing to its excellent strengthening effects. This approach generally employs coherent and nano-sized precipitates, as incoherent precipitates energetically become coarse due to their incompatibility with matrix and provide a negligible strengthening effect or even cause brittleness. Here we propose a shear band-driven dispersion of nano-sized and semicoherent precipitates, which show significant strengthening effects. We add aluminum to a model CoNiV medium-entropy alloy with a face-centered cubic structure to form the L2 Heusler phase with an ordered body-centered cubic structure, as predicted by ab initio calculations. Micro-shear bands act as heterogeneous nucleation sites and generate finely dispersed intragranular precipitates with a semicoherent interface, which leads to a remarkable strength-ductility balance. This work suggests that the structurally dissimilar precipitates, which are generally avoided in conventional alloys, can be a useful design concept in developing high-strength ductile structural materials.© 2021. The Author(s).

Du X H, Li W P, Chang H T, et al.

Dual heterogeneous structures lead to ultrahigh strength and uniform ductility in a Co-Cr-Ni medium-entropy alloy

[J]. Nat. Commun., 2020, 11: 2390

DOI      PMID      [本文引用: 4]

Alloys with ultra-high strength and sufficient ductility are highly desired for modern engineering applications but difficult to develop. Here we report that, by a careful controlling alloy composition, thermomechanical process, and microstructural feature, a Co-Cr-Ni-based medium-entropy alloy (MEA) with a dual heterogeneous structure of both matrix and precipitates can be designed to provide an ultra-high tensile strength of 2.2 GPa and uniform elongation of 13% at ambient temperature, properties that are much improved over their counterparts without the heterogeneous structure. Electron microscopy characterizations reveal that the dual heterogeneous structures are composed of a heterogeneous matrix with both coarse grains (10∼30 μm) and ultra-fine grains (0.5∼2 μm), together with heterogeneous L1-structured nanoprecipitates ranging from several to hundreds of nanometers. The heterogeneous L1 nanoprecipitates are fully coherent with the matrix, minimizing the elastic misfit strain of interfaces, relieving the stress concentration during deformation, and playing an active role in enhanced ductility.

An Z B, Mao S C, Liu Y N, et al.

A novel HfNbTaTiV high-entropy alloy of superior mechanical properties designed on the principle of maximum lattice distortion

[J]. J. Mater. Sci. Technol., 2021, 79: 109

DOI      [本文引用: 4]

This paper reports a synergistic design of high-performance BCC high-entropy alloy based on the combined consideration of the principles of intrinsic ductility of elements, maximum atomic size difference for solid solution strengthening and the valence electron concentration criterion for ductility. The single-phase BCC HfNbTaTiV alloy thus designed exhibited a high compressive yield strength of 1350 MPa and a high compressive ductility of >45 % at the room temperature. This represents a 50 % increase in yield strength relative to a HfNbTaTiZr alloy. This is attributed to the maximized solid solution strengthening effect caused by lattice distortion, which is estimated to be 1094 MPa. The alloy was also able to retain 53 % of its yield strength and 77 % of its ductility at 700 °C. These properties are superior to those of most refractory BCC high-entropy alloys reported in the literature.

Lee C, Chou Y, Kim G, et al.

Lattice-distortion-enhanced yield strength in a refractory high-entropy alloy

[J]. Adv. Mater., 2020, 32: 2004029

DOI      URL    

Feng R, Feng B J, Gao M C, et al.

Superior high-temperature strength in a supersaturated refractory high-entropy alloy

[J]. Adv. Mater., 2021, 33: 2102401

DOI      URL     [本文引用: 1]

Wu Y, Zhang F, Yuan X Y, et al.

Short-range ordering and its effects on mechanical properties of high-entropy alloys

[J]. J. Mater. Sci. Technol., 2021, 62: 214

DOI      [本文引用: 1]

In this letter, we briefly summarize experimental and theoretical findings of formation and characterization of short-range orderings (SROs) as well as their effects on the deformation behavior of high-entropy alloys (HEAs). We show that existence of SROs is a common yet key structural feature of HEAs, and tuning the degree of SROs is an effective way for optimizing mechanical properties of HEAs. In additional, the challenges concerning about formation mechanism and characterization of SROs in HEAs are discussed, and future research activities in this regard are also proposed.

Bu Y Q, Wu Y, Lei Z F, et al.

Local chemical fluctuation mediated ductility in body-centered-cubic high-entropy alloys

[J]. Mater. Today, 2021, 46: 28

DOI      URL    

Yin S, Ding J, Asta M, et al.

Ab initio modeling of the role of local chemical short-range order on the Peierls potential of screw dislocations in body-centered cubic high-entropy alloys

[J]. npj Comput. Mater., 2020, 6: 1

DOI      URL     [本文引用: 1]

Hu Q, Guo S, Guo J L, et al.

Effect of Mo on high-temperature strength of refractory complex concentrated alloys: A perspective of electronegativity difference

[J]. J. Alloys Compd., 2022, 906: 164186

DOI      URL     [本文引用: 1]

Lei Z F, Liu X J, Wu Y, et al.

Enhanced strength and ductility in a high-entropy alloy via ordered oxygen complexes

[J]. Nature, 2018, 563: 546

DOI      URL     [本文引用: 8]

Lilensten L, Couzinié J P, Perrière L, et al.

Study of a bcc multi-principal element alloy: Tensile and simple shear properties and underlying deformation mechanisms

[J]. Acta Mater., 2018, 142: 131

DOI      URL     [本文引用: 1]

Antillon E, Woodward C, Rao S I, et al.

Chemical short range order strengthening in a model FCC high entropy alloy

[J]. Acta Mater., 2020, 190: 29

DOI      URL     [本文引用: 1]

Fernández-Caballero A, Wróbel J S, Mummery P M, et al.

Short-range order in high entropy alloys: Theoretical formulation and application to Mo-Nb-Ta-V-W system

[J]. J. Phase Equilib. Diffus., 2017, 38: 391

DOI      URL    

Li Q J, Sheng H, Ma E.

Strengthening in multi-principal element alloys with local-chemical-order roughened dislocation pathways

[J]. Nat. Commun., 2019, 10: 3563

DOI      URL     [本文引用: 1]

Fantin A, Lepore G O, Manzoni A M, et al.

Short-range chemical order and local lattice distortion in a compositionally complex alloy

[J]. Acta Mater., 2020, 193: 329

DOI      URL    

Jian W R, Xie Z C, Xu S Z, et al.

Effects of lattice distortion and chemical short-range order on the mechanisms of deformation in medium entropy alloy CoCrNi

[J]. Acta Mater., 2020, 199: 352

DOI      URL    

Kostiuchenko T, Ruban A V, Neugebauer J, et al.

Short-range order in face-centered cubic VCoNi alloys

[J]. Phys. Rev. Mater., 2020, 4: 113802

[本文引用: 1]

He Z F, Jia N, Yan H L, et al.

Multi-heterostructure and mechanical properties of N-doped FeMnCoCr high entropy alloy

[J]. Int. J. Plast., 2021, 139: 102965

DOI      URL     [本文引用: 1]

Zhang R P, Zhao S T, Ding J, et al.

Short-range order and its impact on the CrCoNi medium-entropy alloy

[J]. Nature, 2020, 581: 283

DOI      URL     [本文引用: 6]

Su I A, Tseng K K, Yeh J W, et al.

Strengthening mechanisms and microstructural evolution of ductile refractory medium-entropy alloy Hf20Nb10Ti35Zr35

[J]. Scr. Mater., 2022, 206: 114225

DOI      URL     [本文引用: 1]

Gerold V, Karnthaler H P.

On the origin of planar slip in f.c.c. alloys

[J]. Acta Metall., 1989, 37: 2177

DOI      URL     [本文引用: 1]

Hamdi F, Asgari S.

Influence of stacking fault energy and short-range ordering on dynamic recovery and work hardening behavior of copper alloys

[J]. Scr. Mater., 2010, 62: 693

DOI      URL     [本文引用: 1]

Cao B X, Zhao Y L, Yang T, et al.

L12 -strengthened Co-rich alloys for high-temperature structural applications: A critical review

[J]. Adv. Eng. Mater., 2021, 23: 2100453

DOI      URL     [本文引用: 1]

Yang T, Cao B X, Zhang T L, et al.

Chemically complex intermetallic alloys: A new frontier for innovative structural materials

[J]. Mater. Today, 2022, 52: 161

DOI      URL     [本文引用: 1]

Orowan E.

Fracture and strength of solids

[J]. Rep. Prog. Phys., 1949, 12: 185

DOI      URL     [本文引用: 1]

Liang Y J, Wang L J, Wen Y R, et al.

High-content ductile coherent nanoprecipitates achieve ultrastrong high-entropy alloys

[J]. Nat. Commun., 2018, 9: 4063

DOI      URL     [本文引用: 6]

An Z B, Mao S C, Yang T, et al.

Spinodal-modulated solid solution delivers a strong and ductile refractory high-entropy alloy

[J]. Mater. Horiz., 2021, 8: 948

DOI      PMID      [本文引用: 6]

Body-centered-cubic (BCC) refractory high-entropy alloys (RHEAs) are being actively pursued due to their potential to outperform existing superalloys at elevated temperatures. One bottleneck problem, however, is that these RHEAs lack tensile ductility and, hence, processability at room temperature. The strategy previously invoked to sustain ductility in high-strength HEAs is to manage dislocation movements via incorporating dispersed obstacles; this, however, may also have embrittlement ramifications. Here, a new strategy is demonstrated to achieve ductile BCC HfNbTiV, via decomposing the BCC arrangement (β phase) into a β(BCC) + β*(BCC) arrangement via spinodal decomposition, producing chemical composition modulations and, more importantly, elastic strain on a length scale of a few tens of nanometers. The periodically spaced β*, with large lattice distortion, is particularly potent in heightening the ruggedness of the terrain for the passage of dislocations. This makes the motion of dislocations sluggish, causing a traffic jam and cross-slip, facilitating dislocation interactions, multiplication, and accumulation. Wavy dislocations form walls that entangle with slip bands, promoting strain hardening and delocalizing plastic strain. A simultaneous combination of high yield strength (1.1 GPa) and tensile strain to failure (28%) is achieved; these values are among the best reported so far for refractory high-entropy alloys.

Fan L, Yang T, Zhao Y L, et al.

Ultrahigh strength and ductility in newly developed materials with coherent nanolamellar architectures

[J]. Nat. Commun., 2020, 11: 6240

DOI      PMID      [本文引用: 6]

Nano-lamellar materials with ultrahigh strengths and unusual physical properties are of technological importance for structural applications. However, these materials generally suffer from low tensile ductility, which severely limits their practical utility. Here we show that markedly enhanced tensile ductility can be achieved in coherent nano-lamellar alloys, which exhibit an unprecedented combination of over 2 GPa yield strength and 16% uniform tensile ductility. The ultrahigh strength originates mainly from the lamellar boundary strengthening, whereas the large ductility correlates to a progressive work-hardening mechanism regulated by the unique nano-lamellar architecture. The coherent lamellar boundaries facilitate the dislocation transmission, which eliminates the stress concentrations at the boundaries. Meanwhile, deformation-induced hierarchical stacking-fault networks and associated high-density Lomer-Cottrell locks enhance the work hardening response, leading to unusually large tensile ductilities. The coherent nano-lamellar strategy can potentially be applied to many other alloys and open new avenues for designing ultrastrong yet ductile materials for technological applications.

Zhou X L, Feng Z Q, Zhu L L, et al.

High-pressure strengthening in ultrafine-grained metals

[J]. Nature, 2020, 579: 67

DOI      URL     [本文引用: 1]

Wu X L, Zhu Y T.

Heterogeneous materials: A new class of materials with unprecedented mechanical properties

[J]. Mater. Res. Lett., 2017, 5: 527

DOI      URL     [本文引用: 1]

Ma E, Zhu T.

Towards strength-ductility synergy through the design of heterogeneous nanostructures in metals

[J]. Mater. Today, 2017, 20: 323

DOI      URL     [本文引用: 1]

Wu X L, Jiang P, Chen L, et al.

Extraordinary strain hardening by gradient structure

[J]. Proc. Natl. Acad. Sci. USA, 2014, 111: 7197

DOI      URL    

Cheng Z, Zhou H F, Lu Q H, et al.

Extra strengthening and work hardening in gradient nanotwinned metals

[J]. Science, 2018, 362: eaau1925

DOI      URL     [本文引用: 1]

Otto F, Hanold N L, George E P.

Microstructural evolution after thermomechanical processing in an equiatomic, single-phase CoCrFeMnNi high-entropy alloy with special focus on twin boundaries

[J]. Intermetallics, 2014, 54: 39

DOI      URL     [本文引用: 1]

Wu S W, Wang G, Wang Q, et al.

Enhancement of strength-ductility trade-off in a high-entropy alloy through a heterogeneous structure

[J]. Acta Mater., 2019, 165: 444

DOI      URL     [本文引用: 1]

Wang X, Li Y S, Zhang Q, et al.

Gradient structured copper by rotationally accelerated shot peening

[J]. J. Mater. Sci. Technol., 2017, 33: 758

DOI      [本文引用: 1]

A new technology—rotationally accelerated shot peening (RASP), was developed to prepare gradient structured materials. By using centrifugal acceleration principle and large steel balls, the RASP technology can produce much higher impact energy compared to conventional shot peening. As a proof-of-concept demonstration, the RASP was utilized to refine the surface layer in pure copper (Cu) with an average grain size of ~85 nm. The grain size increases largely from surface downwards the bulk, forming an 800 μm thick gradient-structured surface layer and consequently a micro-hardness gradient. The difference between the RASP technology and other established techniques in preparing gradient structured materials is discussed. The RASP technology exhibits a promoting future for large-scale manufacturing of gradient materials.

Tao N R, Wang Z B, Tong W P, et al.

An investigation of surface nanocrystallization mechanism in Fe induced by surface mechanical attrition treatment

[J]. Acta Mater., 2002, 50: 4603

DOI      URL     [本文引用: 1]

Hasan M N, Liu Y F, An X H, et al.

Simultaneously enhancing strength and ductility of a high-entropy alloy via gradient hierarchical microstructures

[J]. Int. J. Plast., 2019, 123: 178

DOI      URL     [本文引用: 5]

Shi P J, Zhong Y B, Li Y, et al.

Multistage work hardening assisted by multi-type twinning in ultrafine-grained heterostructural eutectic high-entropy alloys

[J]. Mater. Today, 2020, 41: 62

DOI      URL     [本文引用: 2]

Wang M L, Lu Y P, Wang T M, et al.

A novel bulk eutectic high-entropy alloy with outstanding as-cast specific yield strengths at elevated temperatures

[J]. Scr. Mater., 2021, 204: 114132

DOI      URL    

Xiong T, Zheng S J, Pang J Y, et al.

High-strength and high-ductility AlCoCrFeNi2.1 eutectic high-entropy alloy achieved via precipitation strengthening in a heterogeneous structure

[J]. Scr. Mater., 2020, 186: 336

DOI      URL    

Shi P J, Ren W L, Zheng T X, et al.

Enhanced strength-ductility synergy in ultrafine-grained eutectic high-entropy alloys by inheriting microstructural lamellae

[J]. Nat. Commun., 2019, 10: 489

DOI      PMID      [本文引用: 1]

Realizing improved strength-ductility synergy in eutectic alloys acting as in situ composite materials remains a challenge in conventional eutectic systems, which is why eutectic high-entropy alloys (EHEAs), a newly-emerging multi-principal-element eutectic category, may offer wider in situ composite possibilities. Here, we use an AlCoCrFeNi EHEA to engineer an ultrafine-grained duplex microstructure that deliberately inherits its composite lamellar nature by tailored thermo-mechanical processing to achieve property combinations which are not accessible to previously-reported reinforcement methodologies. The as-prepared samples exhibit hierarchically-structural heterogeneity due to phase decomposition, and the improved mechanical response during deformation is attributed to both a two-hierarchical constraint effect and a self-generated microcrack-arresting mechanism. This work provides a pathway for strengthening eutectic alloys and widens the design toolbox for high-performance materials based upon EHEAs.

Lu Y P, Dong Y, Guo S, et al.

A promising new class of high-temperature alloys: Eutectic high-entropy alloys

[J]. Sci. Rep., 2014, 4: 6200

DOI      PMID      [本文引用: 1]

High-entropy alloys (HEAs) can have either high strength or high ductility, and a simultaneous achievement of both still constitutes a tough challenge. The inferior castability and compositional segregation of HEAs are also obstacles for their technological applications. To tackle these problems, here we proposed a novel strategy to design HEAs using the eutectic alloy concept, i.e. to achieve a microstructure composed of alternating soft fcc and hard bcc phases. As a manifestation of this concept, an AlCoCrFeNi2.1 (atomic portion) eutectic high-entropy alloy (EHEA) was designed. The as-cast EHEA possessed a fine lamellar fcc/B2 microstructure, and showed an unprecedented combination of high tensile ductility and high fracture strength at room temperature. The excellent mechanical properties could be kept up to 700 degrees C. This new alloy design strategy can be readily adapted to large-scale industrial production of HEAs with simultaneous high fracture strength and high ductility.

Fu Z Q, Jiang L, Wardini J L, et al.

A high-entropy alloy with hierarchical nanoprecipitates and ultrahigh strength

[J]. Sci. Adv., 2018, 4: eaat8712

DOI      URL     [本文引用: 1]

Jia Z Y, Zhang S Z, Huo J T, et al.

Heterogeneous precipitation strengthened non-equiatomic NiCoFeAlTi medium entropy alloy with excellent mechanical properties

[J]. Mater. Sci. Eng., 2022, A834: 142617

[本文引用: 1]

Qin S, Yang M X, Jiang P, et al.

Designing structures with combined gradients of grain size and precipitation in high entropy alloys for simultaneous improvement of strength and ductility

[J]. Acta Mater., 2022, 230: 117847

DOI      URL     [本文引用: 5]

/

〈 〉