| EXFOLIATION CORROSION BEHAVIOR OF T6 TREATED 2090 Al-Li ALLOY IN EXCO SOLUTION AND EIS DURING EXFOLIATION CORROSION EVOLUTION |
| SU Jingxin; ZHANG Zhao; CAO Fahe; ZHANG Jianqing; CAO Chunan |
| Department of Chemistry; Zhejiang University; Hangzhou 310027 |
|
Cite this article:
SU Jingxin; ZHANG Zhao; CAO Fahe; ZHANG Jianqing; CAO Chunan. EXFOLIATION CORROSION BEHAVIOR OF T6 TREATED 2090 Al-Li ALLOY IN EXCO SOLUTION AND EIS DURING EXFOLIATION CORROSION EVOLUTION. Acta Metall Sin, 2005, 41(9): 974-978 .
|
|
|
Abstract Electrochemical impedance spectroscopy (EIS) and in situ microscopic image of T6 peak-aged AA2090 Al-Li alloys in EXCO solution were studied. The localized corrosion form of the alloy during immersion evolved from pitting through intergranular corrosion, exfoliation corrosion (EC) to post EC. EC initiated at big corrosion pits which were formed with inclusion phase as center in pitting stage. The EC blisters propagate from these big pits till the upper layer is
totally lifted. EIS of the initiation stage of
pitting corrosion consists of a high frequency
capacitive arc and a middle-low frequency
inductive arc, and the inductive arc tends to
disappear when pitting corrosion starts to propagate. In the intergranular corrosion stage, the second time constant corresponding to the corroded area can hardly be distinguished in the capacitive part of the EIS. In the stages of EC propagation and
post EC, their EIS consist of two capacitive arcs.
|
|
Received: 18 January 2005
|
|
|
[1] Liu J A, Zhu X W. Light Alloy Fabr Technol, 1996; 24(5): 2 (刘静安,朱献文.轻合金加工技术, 1996;24(5):2) [2] He J P, Chen W L, Xu W, Fan W X. J Nanjing Univ Aeronaut Astronaut, 1999; 31: 575 (何建平,陈文理,许玮,樊蔚勋.南京航空航天大学学报, 1999;31:575) [3] He B, Sun Y C, Fan W X. J Nanjing Univ Aeronaut Astronaut, 1998; 30: 306 (贺斌,孙有朝,樊蔚勋.南京航空航天大学学报,1998;30: 306) [4] ASTM G34-79.Exfoliation Corrosion Susceptibility in 2xxx and 7xxx Series Aluminum Alloys (EXCO test), 1999 [5] Kelly D J, Robinson M J. Corros Sci,1993;49: 787 [6] Habashi M, Bonte E,Galland J, Bodu J J. Corros Sci, 1993; 35: 169 [7] Conde A, de Damborenear J. Electrochim Acta, 1998; 43: 849 [8] Coude A, de Damborenear J. Corros Sci, 2000; 42: 1393 [9] Buchheit R G Jr, Moran J P, Stoner G E. Corrosion, 1990; 46: 610 [10] Garrard W N. Corrosion, 1994, 50: 215 [11] Buchheit R G, Moran J P, Stoner G E. Corrosion,1994; 50: 120 [12] Kumai G, Kusinski J, Thomas G, Devine T M. Corrosion, 1989; 45: 294 [13] Cao C N, Wang J, Lin H C. J Chin Soc Corros Protect, 1989; 9: 261 (曹楚南,王 佳,林海潮.中国腐蚀与防护学报,1989;9: 261) [14] Cao C N, Zhang J Q. An Introduction to Electrochemical Impedance Spectroscopy.Beijing:Science Press, 2002: 177 (曹楚南,张鉴清.电化学阻抗谱导论.北京:科学出版社,2002: 177) |
| No Suggested Reading articles found! |
|
|