Please wait a minute...
Acta Metall Sin  2025, Vol. 61 Issue (10): 1515-1530    DOI: 10.11900/0412.1961.2024.00009
Research paper Current Issue | Archive | Adv Search |
Effect of Heat Treatment on Microstructure and Mechanical Properties of 18Ni300 Maraging Steel Fabricated by Selective Laser Melting
WU Wenwei1,2, XIANG Chao2(), ZHANG Tao2(), ZOU Zhihang2, SUN Yongfei1,2, LIU Jinpeng2, ZHANG Tao2(), HAN En-Hou2,3
1 School of Physics and Materials Science, Guangzhou University, Guangzhou 510006, China
2 Institute of Corrosion Science and Technology, Guangzhou 510530, China
3 School of Materials Science and Engineering, South China University of Technology, Guangzhou 510641, China
Cite this article: 

WU Wenwei, XIANG Chao, ZHANG Tao, ZOU Zhihang, SUN Yongfei, LIU Jinpeng, ZHANG Tao, HAN En-Hou. Effect of Heat Treatment on Microstructure and Mechanical Properties of 18Ni300 Maraging Steel Fabricated by Selective Laser Melting. Acta Metall Sin, 2025, 61(10): 1515-1530.

Download:  HTML  PDF(9726KB) 
Export:  BibTeX | EndNote (RIS)      
Abstract  

Recently, 18Ni300 maraging steel has been widely used for preparing conformal cooling molds via additive manufacturing. The requirements pertaining to the service life of these molds have become more stringent, but whether the microstructures and properties of these molds can meet the service requirements largely depends on the applied heat treatment. This paper studies the effects of two typical heat treatment processes—direct aging and solution aging—on the microstructure and tensile properties of 18Ni300 maraging steel fabricated via selective laser melting. In all prepared specimens, austenite was present and the classical Nishiyama-Wassermann orientation relationship was observed between austenite and the martensitic matrix. Elements in the as-prepared samples were evenly distributed, with obvious molten-pool and cell structures composed mainly of dislocation entanglements. In addition, a small number of long austenite strips appeared at the grain boundaries. Direct aging partially dissolved the cell and molten-pool structures and enriched Ni at some grain boundaries. The direct-aging sample exhibited relatively high austenite content. Meanwhile, the solution-aging sample exhibited a nearly complete martensite structure with evenly distributed elements. In addition, cell and molten-pool structures were almost completely removed and Ni was enriched at some grain boundaries. Further, trace amounts of austenite remained. Austenite retained in the as-prepared samples showed no obvious chemical composition segregation. Austenite present in the direct-aging and solution-aging samples was Ni enriched and confirmed to be of the reverted type. Ni at certain grain boundaries and cell walls was enriched due to cell-wall dissolution during the direct- and solution-aging treatments. Ni enrichment promoted the formation and stability of reverted austenite. Numerous round rod-shaped Ni3Ti intermetallic compounds precipitated from the matrix after both the treatments, greatly increasing the yield strength from (1090 ± 1.5) MPa of the untreated sample to (1854 ± 13.2) MPa and (2059 ± 9.9) MPa of the direct-aging and solution-aging samples, respectively. The strength of the as-prepared samples was mainly contributed by austenite-to-martensitic phase transformation and solid-solution strengthening, while those of the direct- and solution-aging samples were mainly contributed by austenite-to-martensitic phase transformation, solid-solution strengthening, and precipitation strengthening. Moreover, the solution-aging samples exhibited greater precipitation strengthening than the direct-aging samples, mainly owing to the high density and large length-diameter ratio of their precipitates.

Key words:  additive manufacturing      maraging steel      microstructure      heat treatment      austenite     
Received:  12 January 2024     
ZTFLH:  TG142.1+5  
Fund: Youth Innovation Fund of Institute of Corrosion Science and Technology(E1551601)

URL: 

https://www.ams.org.cn/EN/10.11900/0412.1961.2024.00009     OR     https://www.ams.org.cn/EN/Y2025/V61/I10/1515

Fig.1  Morphology of 18Ni300 maraging steel powder (a), powder particle size distribution (D10, D50, and D90 are the particle sizes of the powder at 10%, 50%, and 90% cumulative distribution, respectively) (b), and schematics of tensile specimen dimensions, impact specimen dimensions, and the scanning strategy employed during selective laser melting (SLM) process (unit: mm) (c)
Fig.2  XRD spectra of SLM 18Ni300 samples after different heat treatments (VA—volume fraction of austenite; AB—as-built, DA—direct aging, SA—solution aging; A—austenite, M—martensite)
Fig.3  OM images of SLM 18Ni300 samples after different heat treatments (a-c) XOZ surface images of AB (a), DA (b), and SA (c) samples (d-f) XOY surface images of AB (d), DA (e), and SA (f) samples
Fig.4  Low (a-c) and high (d-f) magnified SEM images of SLM 18Ni300 samples after different heat treatments (GB—grain boundary) (a, d) AB (b, e) DA (c, f) SA
Fig.5  Inverse pole figures (IPFs) (a-c) and phase distribution maps (d-f) of SLM 18Ni300 samples after different heat treatments (a, d) AB (b, e) DA (c, f) SA
Fig.6  TEM characteristics of AB sample
(a) bright-field (BF) image (Inset is the selected area electron diffraction (SAED) pattern)
(b) retained austenite
(c) TEM images and EDS maps (HAADF—high-angle annular dark field)
(d) detailed view of the cell structure
(e) detailed view of the retained austenite (Inset is the SAED pattern)
(f) EDS line scan result of Fig.6e
Fig.7  TEM characteristics of DA sample
(a) BF image (Inset is the SAED pattern)
(b) reverted austenite
(c) TEM images and EDS maps
(d) detailed view of the cell structure
(e) detailed view of the reverted austenite (Inset is the SAED pattern)
(f) EDS-line scan result of Fig.7e
Fig.8  TEM characteristics of SA sample
(a) BF image (Inset is SAED pattern) (b) detailed view of the cell structure (c) TEM images and EDS maps
Fig.9  TEM characteristics of the reverted austenite of SA sample, including BF image (a), TEM image and EDS maps (b), HRTEM image of Fig.9a (c), fast Fourie transform (FFT) of regions d (d) and e (e) in Fig.9c, and FFT of Fig.9c (f)
Fig.10  BF images, HAADF images and EDS maps of the precipitated phase, and the EDS-line scan results of a nanoparticle in the DA (a) and SA (b) samples
Fig.11  HRTEM images (a, c) and corresponding FFT (b, d) of the precipitated phase in DA (a, b) and SA (c, d) samples (The precipitated phases of DA and SA samples are η-Ni3Ti)
Fig.12  Engineering stress-strain curves of SLM 18Ni300 samples after different heat treatments
StateYS / MPaUTS / MPaEl / %Hardness / HRC
AB1090 ± 1.51147 ± 1.514.5 ± 1.436.6 ± 0.6
DA1854 ± 13.21931 ± 8.18.5 ± 1.052.3 ± 0.3
SA2059 ± 9.92114 ± 9.06.0 ± 1.454.7 ± 0.4
Table 1  Mechanical properties of SLM 18Ni300 samples after different heat treatments
Fig.13  Low (a-c) and high (d-f) magnified SEM images of tensile fractures of SLM 18Ni300 samples after different heat treatments (a, d) AB (b, e) DA (c, f) SA
Fig.14  Schematic of microstructure evolution of SLM 18Ni300 samples after different heat treatments
Fig.15  Kernel average misorientation (KAM) statistics of SLM 18Ni300 samples after different heat treatments
(a) AB (b) DA (c) SA
Fig.16  Estimated and experimental results of yield strength of SLM 18Ni300 samples after heat treatments (ΔσMart—phase transformation streng-thening, Δσss—solid solution strengthening, Δσp—precipitation strengthening)
[1] Ma R L, Peng C Q, Wang R C, et al. Progress in selective laser melted aluminum alloy [J]. Chin. J. Nonferrous Met., 2020, 30: 2773
马如龙, 彭超群, 王日初 等. 选区激光熔化铝合金的研究进展 [J]. 中国有色金属学报, 2020, 30: 2773
[2] Xu D, Gao H B, Dong T, et al. Research progress of metal powder for additive manufacturing [J]. Chin. J. Nonferrous Met., 2021, 31: 245
许 德, 高华兵, 董 涛 等. 增材制造用金属粉末研究进展 [J]. 中国有色金属学报, 2021, 31: 245
[3] Wang Y N. Research on composition optimization of maraging steel and its selective laser melting process [D]. Harbin: Harbin Institute of Technology, 2020
王亚男. 马氏体时效钢成分优化及其激光选区熔化成型工艺研究 [D]. 哈尔滨: 哈尔滨工业大学, 2020
[4] Yin S, Chen C Y, Yan X C, et al. The influence of aging temperature and aging time on the mechanical and tribological properties of selective laser melted maraging 18Ni-300 steel [J]. Addit. Manuf., 2018, 22: 592
[5] Li H, Zhao W J, Li R D, et al. Progress on additive manufacturing of maraging steel [J]. Chin. J. Lasers, 2022, 49(14): 1402102
李 虎, 赵伟江, 李瑞迪 等. 增材制造马氏体时效钢的研究进展 [J]. 中国激光, 2022, 49(14): 1402102
[6] Feng X T, Li J M, Geng S, et al. Effect of heat treatment on low-cycle fatigue properties of selective laser melted IN718 at room temperature [J]. Chin. J. Lasers, 2023, 50(16): 1602301
冯星涛, 李健民, 耿 硕 等. 热处理对激光选区熔化IN718合金室温低周疲劳性能的影响 [J]. 中国激光, 2023, 50(16): 1602301
[7] Tan C L, Zhou K S, Ma W Y, et al. Research progress of laser additive manufacturing of maraging steels [J]. Acta Metall. Sin., 2020, 56: 36
doi: 10.11900/0412.1961.2019.00129
谭超林, 周克崧, 马文有 等. 激光增材制造成型马氏体时效钢研究进展 [J]. 金属学报, 2020, 56: 36
doi: 10.11900/0412.1961.2019.00129
[8] Tekin T, Ischia G, Naclerio F, et al. Effect of a direct aging heat treatment on the microstructure and the tensile properties of a 18Ni-300 maraging steel produced by laser powder bed fusion [J]. Mater. Sci. Eng., 2023, A872: 144921
[9] Tan C L, Zhou K S, Ma W Y, et al. Microstructural evolution, nanoprecipitation behavior and mechanical properties of selective laser melted high-performance grade 300 maraging steel [J]. Mater. Des., 2017, 134: 23
[10] Zhao Z J, Dong C F, Kong D C, et al. Influence of pore defects on the mechanical property and corrosion behavior of SLM 18Ni300 maraging steel [J]. Mater. Charact., 2021, 182: 111514
[11] Wang Y N, Luo L S, Liu T, et al. Tuning process parameters to optimize microstructure and mechanical properties of novel maraging steel fabricated by selective laser melting [J]. Mater. Sci. Eng., 2021, A823: 141740
[12] Allam T, Pradeep K G, Köhnen P, et al. Tailoring the nanostructure of laser powder bed fusion additively manufactured maraging steel [J]. Addit. Manuf., 2020, 36: 101561
[13] Bai Y C, Wang D, Yang Y Q, et al. Effect of heat treatment on the microstructure and mechanical properties of maraging steel by selective laser melting [J]. Mater. Sci. Eng., 2019, A760: 105
[14] Paul M J, Muniandy Y, Kruzic J J, et al. Effect of heat treatment on the strength and fracture resistance of a laser powder bed fusion-processed 18Ni-300 maraging steel [J]. Mater. Sci. Eng., 2022, A844: 143167
[15] Kučerová L, Burdová K, Jeníček Š, et al. Effect of solution annealing and precipitation hardening at 250 oC-550 oC on microstructure and mechanical properties of additively manufactured 1.2709 maraging steel [J]. Mater. Sci. Eng., 2021, A814: 141195
[16] Mei X Y, Yan Y, Fu H D, et al. Effect of aging temperature on microstructure evolution and strengthening behavior of L-PBF 18Ni(300) maraging steel [J]. Addit. Manuf., 2022, 58: 103071
[17] Xu Y T, Li W, Du H, et al. Tailoring the metastable reversed austenite from metastable Mn-rich carbides [J]. Acta Mater., 2021, 214: 116986
[18] Soleimani M, Kalhor A, Mirzadeh H. Transformation-induced plasticity (TRIP) in advanced steels: A review [J]. Mater. Sci. Eng., 2020, A795: 140023
[19] Niu M C, Yin L C, Yang K, et al. Synergistic alloying effects on nanoscale precipitation and mechanical properties of ultrahigh-strength steels strengthened by Ni3Ti, Mo-enriched, and Cr-rich co-precipitates [J]. Acta Mater., 2021, 209: 116788
[20] Casati R, Lemke J, Tuissi A, et al. Aging behaviour and mechanical performance of 18-Ni 300 steel processed by selective laser melting [J]. Metals, 2016, 6: 218
[21] Xiang C, Zhang T, Wu W W, et al. Effect of heat treatment on microstructure and mechanical properties of selective laser melting 18Ni300 maraging steel [J]. Chin. J. Lasers, 2024, 51(16):1602302
向 超, 张 涛, 吴文伟 等. 热处理对选区激光熔化18Ni300马氏体时效钢微观组织和力学性能的影响 [J]. 中国激光, 2024, 51(16): 1602302
[22] Wang J, Tao Q, Fan J T, et al. Enhanced mechanical properties of a high-carbon martensite steel processed by heavy warm rolling and tempering [J]. Mater. Sci. Eng., 2023, A872: 144958
[23] Cayron C, Barcelo F, Carlan Y D. The mechanisms of the fcc-bcc martensitic transformation revealed by pole figures [J]. Acta Mater., 2010, 58: 1395
[24] Kučerová L, Zetková I, Jandová A, et al. Microstructural characterisation and in-situ straining of additive-manufactured X3NiCoMoTi 18-9-5 maraging steel [J]. Mater. Sci. Eng., 2019, A750: 70
[25] Bae K, Shin D, Kim J H, et al. Influence of post heat treatment condition on corrosion behavior of 18Ni300 maraging steel manufactured by laser powder bed fusion [J]. Micromachines, 2022, 13: 1977
[26] Kong D C, Dong C F, Wei S L, et al. About metastable cellular structure in additively manufactured austenitic stainless steels [J]. Addit. Manuf., 2021, 38: 101804
[27] Bertsch K M, Meric De Bellefon G, Kuehl B, et al. Origin of dislocation structures in an additively manufactured austenitic stainless steel 316L [J]. Acta Mater., 2020, 199: 19
doi: 10.1016/j.actamat.2020.07.063
[28] Hu B. Study on fine composition regulation and stabilization of retained austenite in low carbon high strength steels [D]. Beijing: University of Science and Technology Beijing, 2022
胡 斌. 低碳高强钢中残余奥氏体的成分精细调控及稳定性研究 [D]. 北京: 北京科技大学, 2022
[29] Song Y S, Liao Y, Li C W, et al. Effects of reversed austenite on the cryogenic impact toughness of 0Cr16Ni5Mo1 super martensitic stainless steel [J]. Acta Metall. Sin., 2025, 61: 687
doi: 10.11900/0412.1961.2023.00100
宋逸思, 廖 瑜, 李传维, 等. 逆转变奥氏体对0Cr16Ni5Mo1超级马氏体不锈钢低温冲击韧性的影响 [J]. 金属学报, 2025, 61: 687
doi: 10.11900/0412.1961.2023.00100
[30] Mai H L, Cui X Y, Scheiber D, et al. The segregation of transition metals to iron grain boundaries and their effects on cohesion [J]. Acta Mater., 2022, 231: 117902
[31] Niu M C, Zhou G, Wang W, et al. Precipitate evolution and strengthening behavior during aging process in a 2.5 GPa grade maraging steel [J]. Acta Mater., 2019, 179: 296
[32] Galindo-Nava E I, Rivera-Díaz-Del-Castillo P E J. Understanding the factors controlling the hardness in martensitic steels [J]. Scr. Mater., 2016, 110: 96
[33] Galindo-Nava E I, Rivera-Díaz-Del-Castillo P E J. A model for the microstructure behaviour and strength evolution in lath martensite [J]. Acta Mater., 2015, 98: 81
[34] Galindo-Nava E I, Rainforth W M, Rivera-Díaz-Del-Castillo P E J. Predicting microstructure and strength of maraging steels: Elemental optimisation [J]. Acta Mater., 2016, 117: 270
[35] Yang T, Chai L J, Wang H, et al. Strength-ductility synergy through tailoring heterostructures of hot-rolled ferritic-martensitic steels containing varying Si contents [J]. Mater. Sci. Eng., 2023, A886: 145712
[36] Mu Y K, He L H, Deng S H, et al. A high-entropy alloy with dislocation-precipitate skeleton for ultrastrength and ductility [J]. Acta Mater., 2022, 232: 117975
[1] WANG Hongying, YAO Zhihao, LI Dayu, GUO Jing, YAO Kaijun, DONG Jianxin. Similarities and Differences of Microstructure and Mechanical Properties Between High γ' Content Powder and Wrought Superalloys[J]. 金属学报, 2025, 61(9): 1364-1374.
[2] TAN Ruohan, SONG Yongfeng, CHEN Chao, LI Dan, CHENG Shu, LI Xiongbing. Mesomechanical Modeling and Experimental Study of Effective Elastic Tensors in Additively Manufactured Titanium Alloys[J]. 金属学报, 2025, 61(9): 1438-1448.
[3] YANG Fan, PEI Shichao, LUO Xinrui, CHEN Yuxiang, LI Ningyu, CHANG Yongqin. Microstructure Evolution and Mechanical Properties of 6061 Aluminum Alloy Fabricated by Friction Stir Additive Manufacturing[J]. 金属学报, 2025, 61(8): 1129-1140.
[4] XIAO Wenlong, ZANG Chenyang, GUO Jintao, FENG Jiawen, MA Chaoli. Two-Stage Aging Process of 7A65 Aluminum Alloy Thick Plate Based on In Situ Resistance Method[J]. 金属学报, 2025, 61(8): 1153-1164.
[5] WU Zewei, YAN Junxiong, HU Li, HAN Xiuzhu. Abnormal Rolling Behavior and Deformation Mechanisms of Bimodal Non-Basal Texture AZ31 Magnesium Alloy Sheet at Medium Temperature[J]. 金属学报, 2025, 61(8): 1165-1173.
[6] ZHANG Mingchuan, XU Qinsi, LIU Yi, CAI Yusheng, MU Yiqiang, REN Dechun, JI Haibin, LEI Jiafeng. Effect of Hot-Pressing Temperature on the Microstructure and Properties of the Diffusion-Bonded Region of TC4 Alloy[J]. 金属学报, 2025, 61(8): 1183-1192.
[7] LI Xue, YU Zheng, XIE Zhiwen, WANG Jinlong, CHEN Minghui, WANG Fuhui. Corrosion Behavior of Heat-Resistant Steels and Its Enamel Coatings in CO2 Atmosphere at 600 oC[J]. 金属学报, 2025, 61(8): 1245-1255.
[8] XIE Xu, WAN Yibo, ZHONG Ming, ZOU Xiaodong, WANG Cong. Optimizing Microstructures and Mechanical Properties of Electro-Gas Welded Metals for EH36 Shipbuilding Steel Treated by CaF2-TiO2 Fluxes[J]. 金属学报, 2025, 61(7): 998-1010.
[9] SUN Huanteng, MA Yunzhu, CAI Qingshan, WANG Jianning, DUAN Youteng, ZHANG Mengxiang. Differential Microstructure Between fcc and bcc Steel Plates Under Hyper-Velocity Impact[J]. 金属学报, 2025, 61(7): 1011-1023.
[10] CAI Xingzhou, LIU Shengjie, ZHANG Yusen, LI Xiaolong, ZHANG Yuhe, ZHANG Wenbin, CHEN Lei, JIN Miao. Effect of Mn Segregation on Mechanical Properties of 0.3C-11Mn-2.7Al-1.8Si-Fe Medium Mn Steel and Its Mechanism[J]. 金属学报, 2025, 61(7): 1024-1034.
[11] WANG Qiang, LI Xiaobing, HAO Junjie, CHEN Bo, ZHANG Bin, ZHANG Erlin, LIU Kui. Solid-State Phase Transformation Behavior of a Novel Ti-Al-Mn-Nb Alloy[J]. 金属学报, 2025, 61(7): 1060-1070.
[12] LI Dayu, YAO Zhihao, ZHAO Jie, DONG Jianxin, GUO Jing, ZHAO Yu. Evolution of Microstructure and Mechanical Properties of FGH4720Li P/M Superalloy Under Near-Service Conditions[J]. 金属学报, 2025, 61(6): 826-836.
[13] HAO Xubang, CHENG Weili, LI Jian, WANG Lifei, CUI Zeqin, YAN Guoqing, ZHAI Kai, YU Hui. Electrochemical Behavior and Discharge Performance of a Low-Alloyed Mg-Ag Alloy as Anode for Mg-Air Battery[J]. 金属学报, 2025, 61(6): 837-847.
[14] LIU Ziru, GUO Qianying, ZHANG Hongyu, LIU Yongchang. Effects of V on the Microstructure Evolution and Hardness Enhancement of Ti2AlNb Alloy[J]. 金属学报, 2025, 61(6): 848-856.
[15] YANG Xiaoyu, MI Zhenli, FANG Xing, LIU Hangrui, MU Wangzhong. Achieving an Excellent Hole Expansion Behavior in Complex Phase Steels by Characteristic Distribution of Martensite-Austenite Constituents[J]. 金属学报, 2025, 61(5): 674-686.