College of Ocean Science and Engineering, Shanghai Maritime University, Shanghai 201306, China
Cite this article:
SHEN Yuanyuan, DONG Yaohua, DONG Lihua, YIN Yansheng. Corrosion Inhibition Effect of Microorganism on 5754 Al Alloy in Seawater. Acta Metall Sin, 2020, 56(12): 1681-1689.
Currently, with the gradual depletion of onshore resources, more efforts are being devoted to both scientific and resource exploitation of the ocean and the deep sea. Compared with the onshore environment, marine habitats are complex and characterized by high hydrostatic pressure, high salinity, and high marine population. The ocean is a unique aquatic environment, and it has a large population of microorganisms. There is a need to exploit the ocean for new energy sources. The significant challenges of exploiting oil, gas, and minerals have forced the people to innovate and develop advanced exploration tools. Al alloys are attractive for use in marine environments due to their low densities, high strengths, good plasticity, excellent electrical and thermal conductivities, and excellent corrosion resistance. The high chloride concentrations and microorganisms in the ocean have a significant effect on the corrosion resistance of many metallic materials. In this work, the corrosion behavior of 5754 Al alloy in seawater containing B.subtilis was investigated. The corrosion rate was analyzed by the weight loss method. The morphologies of the corrosion products and the corrosion profiles were observed by SEM and white light interferometer, respectively. The corrosion products were analyzed by energy dispersive spectroscopy and XRD. Finally, the corrosion mechanism of the Al alloy was studied using electrochemical impedance spectroscopy. The results show that the corrosion rate of the Al alloy in the seawater with B.subtilis was 12.5 mg/(dm2·d), which was only 1/6 times that in the seawater without the bacteria. A protective film comprising of CaMg(CO3)2 was gradually formed on the surface of the alloy in the presence of the bacteria. The bacteria promoted the formation of the CaMg(CO3)2 film, which protected the alloy from the seawater, and consequently, inhibited the pitting corrosion of the Al alloy in the marine environment.
Fig.1 Surface morphologies and composition analyses of 5754 Al alloy
Fig.2 XRD spectra of 5754 Al alloy after soaking for 15 d in two solutions
Fig.3 2D (a, c, e) and 3D (b, d, f) surface profile images of 5754 Al alloy before (a, b), and after immersion for 15 d in sterile (c, d) and inoculated B.subtilis (e, f) seawater (Arrows show the locations of pitting)
Fig.4 EIS of the 5754 Al alloy in seawater without B.subtilis for different immersion time (Z'—real part of impedance, Z''—imaginary part of impedance, Z—impedance, f—frequency)
Fig.5 EIS of the 5754 Al alloy in seawater with B.subtilis for different immersion time
Fig.6 Equivalent circuit diagrams for 5754 Al alloy immersed in seawater with and without B.subtilis for 1 d (a), 5 d, 10 d and 15 d (b) (Rs—electrolyte resistance, Rf—resistance of products film or mixture film, Qf—constant phase element (CPE) of product film or mixture film, Rct—charge transfer resistance, Qdl—CPE of electron transfer reaction)
Time d
Rs Ω·cm2
Qf
Rf Ω·cm2
Qdl
Rct Ω·cm2
χ2
Yf Ω-1·cm-2·snf
nf
Y0 Ω-1·cm-2·sn
n
1
10.79
-
-
-
4.17×10-5
0.907
1.61×105
0.00217
5
9.15
3.07×10-5
0.905
6.99×104
1.34×10-4
0.530
2.28×104
0.00321
10
10.84
2.03×10-5
0.923
3.56×104
1.62×10-4
0.733
1.48×104
0.00410
15
10.66
4.60×10-4
0.724
1.68×102
2.95×10-5
0.948
1.23×104
0.00160
Table 1 Electrochemical fitting parameters of 5754 Al alloy immersed in seawater without bacteria for different time
Time d
Rs Ω·cm2
Qf
Rf Ω·cm2
Qdl
Rct Ω·cm2
χ2
Yf Ω-1·cm-2·snf
nf
Y0 Ω-1·cm-2·sn
n
1
9.34
-
-
-
1.42×10-5
0.912
1.97×105
0.00359
5
9.85
7.60×10-4
0.594
3.28×103
3.39×10-5
0.950
8.81×104
0.00017
10
10.12
3.56×10-4
0.673
4.33×103
3.44×10-5
0.952
1.11×105
0.00294
15
9.35
2.50×10-4
0.687
9.50×103
2.43×10-5
0.984
3.03×105
0.00023
Table 2 Electrochemical fitting parameters of 5754 Al alloy immersed in seawater with bacteria for different time
Fig.7 The sum of Rf and Rct variation of 5754 Al alloy immersed in seawater with and without B.subtilis for different time
[1]
Ezuber H, El-Houd A, El-Shawesh F. A study on the corrosion behavior of aluminum alloys in seawater [J]. Mater. Des., 2008, 29: 801
doi: 10.1016/j.matdes.2007.01.021
[2]
Guan F, Zhai X F, Duan J Z, et al. Influence of sulfate-reducing bacteria on the corrosion behavior of 5052 aluminum alloy [J]. Surf. Coat. Technol., 2017, 316: 171
doi: 10.1016/j.surfcoat.2017.02.057
[3]
Reboul M C, Baroux B. Metallurgical aspects of corrosion resistance of aluminium alloys [J]. Mater. Corros., 2011, 62: 215
[4]
Villanueva M E, Salinas A, Copello G J, et al. Point of zero charge as a factor to control biofilm formation of Pseudomonas aeruginosa in sol-gel derivatized aluminum alloy plates [J]. Surf. Coat. Technol., 2014, 254: 145
doi: 10.1016/j.surfcoat.2014.05.074
[5]
Liang M X, Melchers R, Chaves I. Corrosion and pitting of 6060 series aluminium after 2 years exposure in seawater splash, tidal and immersion zones [J]. Corros. Sci., 2018, 140: 286
doi: 10.1016/j.corsci.2018.05.036
[6]
Donatus U, Thompson G E, Omotoyinbo J A, et al. Corrosion pathways in aluminium alloys [J]. Trans. Nonferrous Met. Soc., 2017, 27: 55
doi: 10.1016/S1003-6326(17)60006-2
[7]
Batmanghelich F, Li L, Seo Y. Influence of multispecies biofilms of Pseudomonas aeruginosa and Desulfovibrio vulgaris on the corrosion of cast iron [J]. Corros. Sci., 2017, 121: 94
doi: 10.1016/j.corsci.2017.03.008
[8]
Zhou E Z, Li H B, Yang C T, et al. Accelerated corrosion of 2304 duplex stainless steel by marine Pseudomonas aeruginosa biofilm [J]. Int. Biodeter. Biodegr., 2018, 127: 1
doi: 10.1016/j.ibiod.2017.11.003
[9]
Little B J, Lee J S, Ray R I. The influence of marine biofilms on corrosion: A concise review [J]. Electrochim. Acta, 2008, 54: 2
doi: 10.1016/j.electacta.2008.02.071
[10]
Wang H, Ju L K, Castaneda H, et al. Corrosion of carbon steel C1010 in the presence of iron oxidizing bacteria Acidithiobacillus ferrooxidans [J]. Corros. Sci., 2014, 89: 250
doi: 10.1016/j.corsci.2014.09.005
[11]
Dou W W, Jia R, Jin P, et al. Investigation of the mechanism and characteristics of copper corrosion by sulfate reducing bacteria [J]. Corros. Sci., 2018, 144: 237
doi: 10.1016/j.corsci.2018.08.055
[12]
Jia R, Yang D Q, Xu J, et al. Microbiologically influenced corrosion of C1018 carbon steel by nitrate reducing Pseudomonas aeruginosa biofilm under organic carbon starvation [J]. Corros. Sci., 2017, 127: 1
doi: 10.1016/j.corsci.2017.08.007
[13]
Homborg A M, Leon M C F, Tinga T, et al. Detection of microbiologically influenced corrosion by electrochemical noise transients [J]. Electrochim. Acta, 2014, 136: 223
doi: 10.1016/j.electacta.2014.05.102
[14]
Giacobone A F F, Rodriguez S A, Burkart A L, et al. Microbiological induced corrosion of AA 6061 nuclear alloy in highly diluted media by Bacillus cereus RE 10 [J]. Int. Biodeter. Biodegr., 2011, 65: 1161
doi: 10.1016/j.ibiod.2011.08.012
[15]
Moradi M, Song Z L, Yang L J, et al. Effect of marine Pseudoalteromonas sp. on the microstructure and corrosion behaviour of 2205 duplex stainless steel [J]. Corros. Sci., 2014, 84: 103
doi: 10.1016/j.corsci.2014.03.018
[16]
Mansfeld F, Hsu H, Örnek D, et al. Corrosion control using regenerative biofilms on aluminum 2024 and brass in different media [J]. J. Electrochem. Soc., 2002, 149: B130
doi: 10.1149/1.1456922
[17]
Jayaraman A, Ornek D, Duarte D A, et al. Axenic aerobic biofilms inhibit corrosion of copper and aluminum [J]. Appl. Microbiol. Biotechnol., 1999, 52: 787
doi: 10.1007/s002530051592
pmid: 10616712
[18]
Jia R, Yang D Q, Xu D K, et al. Electron transfer mediators accelerated the microbiologically influence corrosion against carbon steel by nitrate reducing Pseudomonas aeruginosa biofilm [J]. Bioelectrochemistry, 2017, 118: 38
doi: 10.1016/j.bioelechem.2017.06.013
pmid: 28715664
[19]
Weiner S, Dove P M. An overview of biomineralization processes and the problem of the vital effect [J]. Rev. Mineral. Geochem., 2003, 54: 1
doi: 10.2113/0540001
[20]
Dejong J T, Mortensen B M, Martinez B C, et al. Bio-mediated soil improvement [J]. Ecol. Eng., 2010, 36: 197
doi: 10.1016/j.ecoleng.2008.12.029
[21]
Uad I, Gonzalez-Lopez J, Silva-Castro A G, et al. Precipitation of carbonates crystals by bacteria isolated from a submerged fixed-film bioreactor used for the treatment of urban wastewater [J]. Int. J. Environ. Res., 2014, 8: 435
[22]
Liu H W, Gu T Y, Zhang G A, et al. The effect of magneticfield on biomineralization and corrosion behavior of carbon steel induced by iron-oxidizing bacteria [J]. Corros. Sci., 2016, 102: 93
doi: 10.1016/j.corsci.2015.09.023
[23]
Konhauser K O. Diversity of bacterial iron mineralization [J]. Earth-Sci. Rev., 1998, 43: 91
doi: 10.1016/S0012-8252(97)00036-6
[24]
Abraham W R, Nogales B, Golyshin P N, et al. Polychlorinated biphenyl-degrading microbial communities in soils and sediments [J]. Curr. Opin. Microbiol., 2002, 5: 246
doi: 10.1016/s1369-5274(02)00323-5
pmid: 12057677
[25]
Liu T, Guo Z W, Zeng Z S, et al. Marine bacteria provide lasting anticorrosion activity for steel via biofilm-induced mineralization [J]. ACS Appl. Mater. Interfaces, 2018, 10: 40317
doi: 10.1021/acsami.8b14991
pmid: 30335931
[26]
Lewis A C, Heard P J. The effects of calcium phosphate deposition upon corrosion of CoCr alloys and the potential for implant failure [J]. J. Biomed. Mater. Res., 2005, 75A: 365
doi: 10.1002/(ISSN)1552-4965
[27]
Abdel-Gawad S A, Osman W M, Fekry A M. Characterization and corrosion behavior of anodized aluminum alloys for military industries applications in artificial seawater [J]. Surf. Interfaces, 2019, 14: 314
[28]
Acosta G, Veleva L, López J L, et al. Contrasting initial events of localized corrosion on surfaces of 2219-T42 and 6061-T6 aluminum alloys exposed in Caribbean seawater [J]. Trans. Nonferrous Met. Soc. China, 2019, 29: 34
doi: 10.1016/S1003-6326(18)64912-X