Please wait a minute...
金属学报  2026, Vol. 62 Issue (8): 1395-1404    DOI: 10.11900/0412.1961.2024.00239
  研究论文 本期目录 | 过刊浏览 |
基于固溶元素增材制造镍基高温合金的成分设计
张雪1,2, 梁静静2(), 赵玉淞3, 章环2, 穆亚航1,2, 周亦胄2, 孙晓峰2, 李金国2()
1 中国科学技术大学 材料科学与工程学院 沈阳 110016
2 中国科学院金属研究所 师昌绪先进材料创新中心 沈阳 110016
3 沈阳航空航天大学 材料科学与工程学院 沈阳 110136
Design of Additively Manufactured Ni-Based Superalloys Based on Solid Solution Elements
ZHANG Xue1,2, LIANG Jingjing2(), ZHAO Yusong3, ZHANG Huan2, MU Yahang1,2, ZHOU Yizhou2, SUN Xiaofeng2, LI Jinguo2()
1 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
2 Shi -changxu Innovation Center for Advanced Materials, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
3 School of Materials Science and Engineering, Shenyang Aerospace University, Shenyang 110136, China
引用本文:

张雪, 梁静静, 赵玉淞, 章环, 穆亚航, 周亦胄, 孙晓峰, 李金国. 基于固溶元素增材制造镍基高温合金的成分设计[J]. 金属学报, 2026, 62(8): 1395-1404.
Xue ZHANG, Jingjing LIANG, Yusong ZHAO, Huan ZHANG, Yahang MU, Yizhou ZHOU, Xiaofeng SUN, Jinguo LI. Design of Additively Manufactured Ni-Based Superalloys Based on Solid Solution Elements[J]. Acta Metall Sin, 2026, 62(8): 1395-1404.

全文: PDF(4141 KB)   HTML
摘要: 

易形成裂纹和高温强度不足是增材制造镍基高温合金面临的重大难题,基于固溶元素的成分设计是解决这两大难题的有效途径之一。本工作结合热力学计算,通过OM、XRD、SEM、TEM以及拉伸实验测试分析了增材制造镍基高温合金中γ'相含量、裂纹、错配度和拓扑密排(TCP)相析出情况。结果表明,ZGH-10合金的固溶强度为236 MPa,裂纹面积分数为(1.3 × 10-4)%;错配度为-0.26%,γ'相为方形。在1000 ℃下热暴露500 h时,ZGH-10合金中无TCP相析出。在25、760和1000 ℃下,ZGH-10合金的抗拉强度分别为1290、1089和555 MPa,延伸率分别为17.0%、10.8%和28.5%,表现出优异的强度与塑性。

关键词 : 增材制造,  镍基高温合金,  固溶元素,  成分设计    
Abstract:

Cracking and insufficient strength at high temperatures are major challenges in the manufacturing of additive-manufactured nickel-based superalloys, but can be effectively solved by a composition design based on solid solution elements. In this study, the amounts of γ′ phases, cracks, lattice mismatch, and topological close-packed (TCP) phase in additively manufactured Ni-based superalloys were investigated through thermodynamic calculations, OM, XRD, SEM,TEM, and tensile property tests. The preliminarily optimized ZGH-10 alloy exhibited a good microstructure and excellent tensile properties, with a solid solution strength and crack area percentage of 236 MPa and (1.3 × 10-4)%, respectively. The lattice mismatch of the ZGH-10 alloy (-0.26%) contributes to square γ' phases. After thermal exposure to 1000 oC for 500 h, no TCP phase precipitation appears in the ZGH-10 alloy. At 25 oC, 760 oC, and 1000 oC, the ZGH-10 alloy delivers tensile strengths of 1290, 1089, and 555 MPa, respectively, and elongations of 17.0%, 10.8%, and 28.5%, respectively, showing excellent strength and ductility of the alloy.

Key words: additive manufacturing    Ni-based superalloy    solid solution element    composition design
收稿日期: 2024-07-17     
ZTFLH:  TG142  
基金资助:国家科技重大专项项目(Y2019-VII-0011-0151);国家重点研发计划项目(2021YFB3702503)
通讯作者: 李金国,jgli@imr.ac.cn,主要从事高温合金材料研制与构件制备研究; 梁静静,jjliang@imr.ac.cn,主要从事增材制造高温合金材料研发与工艺优化研究
Corresponding author: LI Jinguo, professor, Tel: (024)83978872, E-mail: jgli@imr.ac.cn; LIANG Jingjing, professor, Tel: (024)23971787, E-mail: jjliang@imr.ac.cn
作者简介: 张 雪,女,1995年生,博士生
LevelCoCrWMoRe
18.05.05.00.00.0
210.07.57.52.53.0
312.010.010.05.06.0
表1  5因素3水平正交表 (mass fraction / %)
AlloyCoCrWMoRe
ZGH-18.010.07.50.00.0
ZGH-210.010.05.00.03.0
ZGH-38.07.510.00.00.0
ZGH-412.010.05.02.50.0
ZGH-510.07.55.00.06.0
ZGH-612.05.010.00.03.0
ZGH-712.05.07.50.06.0
ZGH-812.07.55.05.00.0
ZGH-98.07.57.52.53.0
ZGH-1010.05.07.55.00.0
ZGH-118.05.05.02.56.0
ZGH-128.05.05.05.03.0
表2  镍基高温合金中固溶元素的名义成分 (mass fraction / %)
图1  合金粉末形貌和粒径分布
图2  激光能量沉积后用于拉伸测试样品实物图和拉伸试样的尺寸
图3  Thermo-Calc计算的合金在760和1000 ℃下的γ'相含量
Elementki MPa∙At. Fraction-1/2Md valueeV
Al2251.900
Ti7752.271
Ta11912.224
Co39.40.777
Cr3371.142
W9771.655
Mo10151.550
Re10001.267
C1061-
表3  镍基高温合金中各元素固溶强化系数和合金元素的d轨道能级(Md)[16,20]
图4  ZGH-1和ZGH-10合金中纵截面的裂纹分布情况
图5  合金固溶强度与裂纹面积分数的关系
图6  ZGH-11合金中的液化裂纹
图7  室温下ZGH-8和ZGH-10合金(002)峰XRD谱以及分峰后的拟合曲线
Alloyaγ' / nmaγ / nmδ / %
ZGH-80.357060.35751-0.13
ZGH-100.357760.35870-0.26
表4  ZGH-8和ZGH-10合金γ/γ'相的晶格常数和错配度
图8  ZGH-8和ZGH-10合金γ'相暗场TEM像
图9  ZGH-10合金在1000 ℃下热暴露100和500 h碳化物的类型及面扫描结果和电子衍射花样
图10  ZGH-10合金在1000 ℃下热暴露500 h后析出的MC碳化物的SEM像及元素面扫描分布图
图11  ZGH-10合金拉伸性能及与其目前增材镍基高温合金[28~31]的对比
图12  ZGH-10合金在不同温度下拉伸断口形貌的SEM像
图13  ZGH-10合金拉伸变形后显微组织的TEM像
图14  Lomer-Cottrell (LC)锁形成示意图
[1] Zhang Z X, Yu J J, Liu J L. Anisotropy of stress rupture property of Ni base single crystal superalloy DD432 [J]. Acta Metall. Sin., 2023, 59: 1559
[1] 张子轩, 于金江, 刘金来. 镍基单晶高温合金DD432的持久性能各向异性 [J]. 金属学报, 2023, 59: 1559
[2] Zhang J, Wang L, Xie G, et al. Recent progress in research and development of nickel-based single crystal superalloys [J]. Acta Metall. Sin., 2023, 59: 1109
[2] 张 健, 王 莉, 谢 光 等. 镍基单晶高温合金的研发进展 [J]. 金属学报, 2023, 59: 1109
[3] Sun X F, Song W, Liang J J, et al. Research and development in materials and processes of superalloy fabricated by laser additive manufacturing [J]. Acta Metall. Sin., 2021, 57: 1471
[3] 孙晓峰, 宋 巍, 梁静静 等. 激光增材制造高温合金材料与工艺研究进展 [J]. 金属学报, 2021, 57: 1471
[4] Hu Y L, Lin X, Li Y L, et al. Effect of heat treatment on the microstructural evolution and mechanical properties of GH4099 additive-manufactured by directed energy deposition [J]. J. Alloys Compd., 2019, 800: 163
[5] Guo C, Li G, Li S, et al. Additive manufacturing of Ni-based superalloys: Residual stress, mechanisms of crack formation and strategies for crack inhibition [J]. Nano Mater. Sci., 2023, 5: 53
[6] Murakumo T, Kobayashi T, Koizumi Y, et al. Creep behaviour of Ni-base single-crystal superalloys with various γ′ volume fraction [J]. Acta Mater., 2004, 52: 3737
[7] Cloots M, Uggowitzer P J, Wegener K. Investigations on the microstructure and crack formation of IN738LC samples processed by selective laser melting using Gaussian and doughnut profiles [J]. Mater. Des., 2016, 89: 770
[8] Lopez-Galilea I, Ruttert B, He J Y, et al. Additive manufacturing of CMSX-4 Ni-base superalloy by selective laser melting: Influence of processing parameters and heat treatment [J]. Addit. Manuf., 2019, 30: 100874
[9] Taheri M, Razavi M, Kashani-Bozorg S F, et al. Relationship between solidification and liquation cracks in the joining of GTD-111 nickel-based superalloy by Nd: YAG pulsed-laser welding [J]. J. Mater. Res. Technol., 2021, 15: 5635
[10] Lu N N, Guo Y M, Yang S L, et al. Formation mechanisms of hot cracks in laser additive repairing single crystal superalloys [J]. Acta Metall. Sin., 2023, 59: 1243
[10] 卢楠楠, 郭以沫, 杨树林 等. 激光增材修复单晶高温合金的热裂纹形成机制 [J]. 金属学报, 2023, 59: 1243
[11] Ren W J, Lu F G, Yang R J, et al. Liquation cracking in fiber laser welded joints of Inconel 617 [J]. J. Mater. Process. Technol., 2015, 226: 214
[12] Chauvet E, Kontis P, Jägle E A, et al. Hot cracking mechanism affecting a non-weldable Ni-based superalloy produced by selective electron beam melting [J]. Acta Mater., 2018, 142: 82
[13] Adegoke O, Andersson J, Brodin H, et al. Influence of laser powder bed fusion process parameters on the microstructure and cracking susceptibility of nickel-based superalloy alloy 247LC [J]. Results Mater., 2022, 13: 100256
[14] Divya V D, Muñoz-Moreno R, Messé O M D M, et al. Microstructure of selective laser melted CM247LC nickel-based superalloy and its evolution through heat treatment [J]. Mater. Charact., 2016, 114: 62
[15] Song W, Yang J Y, Liang J J, et al. A new approach to design advanced superalloys for additive manufacturing [J]. Addit. Manuf., 2024, 84: 104098
[16] Harrison N J, Todd I, Mumtaz K. Reduction of micro-cracking in nickel superalloys processed by Selective Laser Melting: A fundamental alloy design approach [J]. Acta Mater., 2015, 94: 59
[17] Zhang X, Mu Y H, Lu N N, et al. Effect of solid solution elements on cracking susceptibility of Ni-based superalloys during additive manufacturing [J]. J. Mater. Sci. Technol., 2024, 190: 218
[18] Ur Rehman H, Durst K, Neumeier S, et al. On the temperature dependent strengthening of nickel by transition metal solutes [J]. Acta Mater., 2017, 137: 54
[19] Chen J B, Chen J Y, Wang Q J, et al. Mutation in TCP phases and superior stress rupture life led by W/Mo ratio in Ni-based single crystal superalloys [J]. Mater. Lett., 2022, 312: 131656
[20] Reed R C, Tao T, Warnken N. Alloys-By-Design: Application to nickel-based single crystal superalloys [J]. Acta Mater., 2009, 57: 5898
[21] Zhang X, Mu Y H, Ma L, et al. Cracking on a nickel-based superalloy fabricated by direct energy deposition [J]. China Foundry, 2024, 21: 311
[22] Liang Z D, Neumeier S, Rao Z Y, et al. CALPHAD informed design of multicomponent CoNiCr-based superalloys exhibiting large lattice misfit and high yield stress [J]. Mater. Sci. Eng., 2022, A854: 143798
[23] Zhang J X, Wang J C, Harada H, et al. The effect of lattice misfit on the dislocation motion in superalloys during high-temperature low-stress creep [J]. Acta Mater., 2005, 53: 4623
[24] Christofidou K A, Jones N G, Pickering E J, et al. The microstructure and hardness of Ni-Co-Al-Ti-Cr quinary alloys [J]. J. Alloys Compd., 2016, 688: 542
[25] Rae C M F, Reed R C. The precipitation of topologically close-packed phases in rhenium-containing superalloys [J]. Acta Mater., 2001, 49: 4113
[26] Seiser B, Drautz R, Pettifor D G. TCP phase predictions in Ni-based superalloys: Structure maps revisited [J]. Acta Mater., 2011, 59: 749
[27] Liu J L, Sun J X, Meng J, et al. Microstructural stability and stress rupture properties of a third-generation Ni base single crystal supalloy [J]. Acta Metall. Sin., 2024, 60: 770
[27] 刘金来, 孙晶霞, 孟 杰 等. 一种第三代单晶高温合金的组织稳定性与持久性能 [J]. 金属学报, 2024, 60: 770
[28] Zhou W Z, Tian Y S, Tan Q B, et al. Effect of carbon content on the microstructure, tensile properties and cracking susceptibility of IN738 superalloy processed by laser powder bed fusion [J]. Addit. Manuf., 2022, 58: 103016
[29] Ma L, Kong X W, Liang J J, et al. Influence of pulsed laser scanning patterns on microstructural evolution and mechanical properties of Inconel 718 in direct laser deposition [J]. J. Mater. Res. Technol., 2023, 25: 1231
[30] Tang Y T, Panwisawas C, Ghoussoub J N, et al. Alloys-by-design: Application to new superalloys for additive manufacturing [J]. Acta Mater., 2021, 202: 417
[31] Li Y, Liang X Y, Yu Y F, et al. Microstructures and mechanical properties evolution of IN939 alloy during electron beam selective melting process [J]. J. Alloys Compd., 2021, 883: 160934
[32] Long H B, Liu Y N, Kong D L, et al. Shearing mechanisms of stacking fault and anti-phase-boundary forming dislocation pairs in the γ′ phase in Ni-based single crystal superalloy [J]. J. Alloys Compd., 2017, 724: 287
[33] Jiang W, Gao X Z, Guo Y Z, et al. Dynamic impact behavior and deformation mechanisms of Cr26Mn20Fe20Co20Ni14 high-entropy alloy [J]. Mater. Sci. Eng., 2021, A824: 141858
[34] Xu X D, Liu P, Tang Z, et al. Transmission electron microscopy characterization of dislocation structure in a face-centered cubic high-entropy alloy Al0.1CoCrFeNi [J]. Acta Mater., 2018, 144: 107
[35] Song Y L, Fan J K, Li J Y, et al. New insights into the optimisation of the solution heat treatment process and properties of CMSX-4 superalloys [J]. Mater. Sci. Eng., 2024, A890: 145947
[36] Zhang J X, Murakumo T, Harada H, et al. Dependence of creep strength on the interfacial dislocations in a fourth generation SC superalloy TMS-138 [J]. Scr. Mater., 2003, 48: 287
[1] 彭望君, 王长河, 杜大帆, 董安平, 陈彪, 孙宝德. 激光粉末床熔融镍基高温合金中第二相演化机制与调控策略进展[J]. 金属学报, 2026, 62(7): 1147-1162.
[2] 史玉升, 程焜, 张程健, 卢佳浩, 李伟, 张李超, 魏青松, 蔡超. 难加工金属增材制造/热等静压融合成形研究现状与展望[J]. 金属学报, 2026, 62(5): 770-784.
[3] 崔天亮, 谢兴飞, 温晓灿, 吕少敏, 曲敬龙, 杜金辉. GH4151难变形高温合金的拉伸行为及其断裂失效机制[J]. 金属学报, 2026, 62(3): 445-457.
[4] 赵晓, 徐超, 江河, 姚志浩, 董建新. GH4738镍基高温合金O累积程度对疲劳性能与晶界损伤的影响及表征[J]. 金属学报, 2026, 62(2): 328-338.
[5] 闫静, 张佳丽, 邓睿, 何洋, 文新理, 章清泉, 乔利杰. Sc在镍基变形高温合金BYG36真空感应熔炼中的烧损机制[J]. 金属学报, 2026, 62(2): 363-371.
[6] 李文亚, 杨景文, 雒晓涛, 殷硕, 徐雅欣. 影响冷喷涂粒子沉积的关键因素:粉末表面氧化综述[J]. 金属学报, 2026, 62(1): 17-28.
[7] 马成勇, 侯旭儒, 赵琳, 阚成玲, 曹洋, 彭云, 田志凌. 电弧增材制造高强度Al-Mg-Sc系合金研究进展:冶金缺陷、微观组织和力学性能[J]. 金属学报, 2026, 62(1): 29-46.
[8] 刘海滨, 张迎星, 谢瑞山, 陈树君. 固相摩擦增材制造技术研究进展及其应用现状[J]. 金属学报, 2026, 62(1): 100-116.
[9] 谭若涵, 宋永锋, 陈超, 李丹, 成庶, 李雄兵. 增材制造钛合金等效弹性张量的细观力学建模与实验研究[J]. 金属学报, 2025, 61(9): 1438-1448.
[10] 杨帆, 裴世超, 罗新蕊, 陈宇翔, 李宁宇, 常永勤. 6061铝合金搅拌摩擦增材制造显微组织演变及力学性能[J]. 金属学报, 2025, 61(8): 1129-1140.
[11] 谢信亮, 周丽萍, 余建波, 玄伟东, 陈超越, 王江, 任忠鸣. 横向弱磁场对镍基高温合金发散双晶竞争生长行为的影响[J]. 金属学报, 2025, 61(8): 1203-1216.
[12] 周一鸣, 韩勇军, 谢光, 郑伟, 肖炎彬, 潘阳, 张健. 一种镍基高温合金的高温HCl腐蚀行为[J]. 金属学报, 2025, 61(5): 770-782.
[13] 黄科, 李新志, 方学伟, 卢秉恒. 镁合金电弧熔丝增材制造技术研究现状与展望[J]. 金属学报, 2025, 61(3): 397-419.
[14] 韩启飞, 狄兴隆, 郭跃岭, 叶水俊, 郑元翾, 刘长猛. 电弧熔丝增材制造Mg/Mg双金属的组织与力学性能[J]. 金属学报, 2025, 61(2): 211-225.
[15] 周生玉, 胡明昊, 李冲, 丁海民, 郭乾应, 刘永长. 一种 γ'/γ'' 相强化镍基高温合金的蠕变行为[J]. 金属学报, 2025, 61(2): 226-234.