Please wait a minute...
金属学报  2022, Vol. 58 Issue (7): 943-955    DOI: 10.11900/0412.1961.2020.00531
  研究论文 本期目录 | 过刊浏览 |
辐照条件下Fe-Cu合金中富Cu析出相的临界形核尺寸和最小能量路径的弦方法计算
刘续希1, 柳文波1(), 李博岩2, 贺新福3, 杨朝曦1, 恽迪1
1.西安交通大学 核科学与技术学院 西安 710049
2.清华大学 材料学院 北京 100084
3.中国原子能科学研究院 北京 102413
Calculation of Critical Nucleus Size and Minimum Energy Path of Cu-Riched Precipitates During Radiation in Fe-Cu Alloy Using String Method
LIU Xuxi1, LIU Wenbo1(), LI Boyan2, HE Xinfu3, YANG Zhaoxi1, YUN Di1
1.School of Nuclear Science and Technology, Xi'an Jiaotong University, Xi'an 710049, China
2.School of Materials Science and Engineering, Tsinghua University, Beijing 100084, China
3.China Institute of Atomic Energy, Beijing 102413, China
引用本文:

刘续希, 柳文波, 李博岩, 贺新福, 杨朝曦, 恽迪. 辐照条件下Fe-Cu合金中富Cu析出相的临界形核尺寸和最小能量路径的弦方法计算[J]. 金属学报, 2022, 58(7): 943-955.
Xuxi LIU, Wenbo LIU, Boyan LI, Xinfu HE, Zhaoxi YANG, Di YUN. Calculation of Critical Nucleus Size and Minimum Energy Path of Cu-Riched Precipitates During Radiation in Fe-Cu Alloy Using String Method[J]. Acta Metall Sin, 2022, 58(7): 943-955.

全文: PDF(2593 KB)   HTML
摘要: 

基于约束弦方法和相场理论,对辐照条件下Fe-Cu合金中富Cu析出相的临界形核尺寸和最小能量路径进行了计算,得到了不同温度和不同Cu含量的富Cu团簇的最小能量路径、临界形核半径、空位浓度场分布等参数。计算结果表明:温度和Cu含量对Fe-Cu二元合金中富Cu相的析出过程的能量路径和临界形核团簇尺寸有很大影响。温度是影响形核能量路径方向的主要因素,Cu含量是影响团簇生长速率的主要因素。温度越高,Cu含量越高,形核达到临界形核尺寸所需要的时间越短,所需要翻越的能量势垒越低。Cu元素浓度场的分布对辐照空位浓度的分布有很大的影响。在富Cu团簇中的空位浓度比Fe-Cu基体中更低,而且Cu浓度越高,空位的浓度越低。上述计算结果与实验结果基本一致。

关键词 : Fe-Cu合金,  相场方法,  约束条件弦方法,  辐照加速析出,  临界形核尺寸    
Abstract:

As a pressure containment shell that supports all components in the nuclear reactor, reactor pressure vessel (RPV) is an irreplaceable core component during the whole life of nuclear power plant. Cu-riched particles precipitated in the early stage of radiation have significant effects on the mechanical property (such as radiation hardening and embrittlement) changes during the application of RPV steel. However, the Cu-riched precipitate with extremely small size (smaller than 2 nm) cannot be detected by the conventional experimental method, such as scanning electron microscope and transmission electron microscope. Hence, it is essential to calculate the critical nucleus size of Cu-riched precipitate under radiation in RPV steel. In this study, based on the constrained string method and phase-field theory, the critical nucleus size and minimum energy path of Cu-riched precipitate in Fe-Cu alloy under irradiation were calculated, and the minimum energy path, critical nucleus radius, and vacancy concentration distribution were also studied. The calculated results showed that both temperature and Cu concentration have a great influence on the energy path and critical nucleus cluster size of Cu-riched particles in Fe-Cu binary alloy. Temperature is the main factor influencing the energy path direction of the nucleus, while Cu concentration is the main factor influencing the growth rate of the nucleus radius. With the increase of temperature, the Cu concentration in the nucleus increases, while the time needed for the Cu-riched particles to reach its critical nucleus size decreases, and the energy barrier needed to be crossed also decreases. The distribution of Cu concentration also has a great influence on the distribution of vacancy during radiation. The vacancy concentration in the Cu-riched cluster is lower than that in the Fe-Cu matrix. The vacancy concentration decreased as the Cu concentration increased. The calculated results are consistent with the experimental results.

Key words: Fe-Cu alloy    phase-field method    constrained string method    radiation-enhanced precipitate    critical nucleus size
收稿日期: 2020-12-30     
ZTFLH:  TG142  
基金资助:国家自然科学基金项目(U1830124);国家自然科学基金项目(11705137);中国博士后科学基金项目(2019M663738);中国核工业集团有限公司领创科研项目
作者简介: 刘续希,男,2000年生,硕士生
图1  形核过程鞍点示意图
Elementα1α2α3α4βγL
Cu6242.2122.833-23.5902-0.004761-5.9197000038022.8
Fe1225.7124.134-23.5143-0.004397-5.89277358.538022.8
表1  Fe-Cu合金Gibbs自由能参数[18,28,30]
ParameterValueUnit
κCu5 × 10-15J·m2·mol-1
κV1 × 10-15J·m2·mol-1
εCu122.833
εV124.134
表2  Fe-Cu合金的界面能参数与本征应变系数[28,29]
T / KDFe / (m2·s-1)DCu / (m2·s-1)MFe / (mol·m·s·kg-1)MCu / (mol·m·s·kg-1)
5507.2 × 10-325.0 × 10-296.7 × 10-174.6 × 10-14
6504.2 × 10-278.0 × 10-253.9 × 10-127.4 × 10-10
表3  不同温度下扩散系数及迁移率的取值[29,35]
图2  650 K时Fe-0.3%Cu合金在辐照强度0.01 dpa/s下演化2步和50步后的能量路径
图3  650 K和0.01 dpa/s下Fe-0.3%Cu演化2步和50步后临界团簇的Cu元素浓度分布和团簇形貌
图4  不同温度下演化50步后Fe-0.3%Cu合金的最小能量路径
图5  不同温度下演化50步后Fe-0.3%Cu合金临界团簇的Cu元素浓度分布和团簇形貌
T / KRC / nmCC / %
5501.72245.4355
6001.76247.8542
6501.79450.2122
7001.82152.5147
表4  不同温度下演化50步后Fe-0.3%Cu合金临界团簇半径与浓度计算结果
图6  不同温度下演化50步后Fe-0.3%Cu合金临界团簇Cu元素浓度的一维分布曲线
图7  650 K下演化50步后不同Cu元素浓度Fe-Cu合金的最小能量路径
图8  650 K下演化50步后不同Cu元素元素浓度Fe-Cu合金临界团簇的Cu元素浓度分布和团簇形貌
AlloyRC / nmCC / %
Fe-0.05Cu1.19026.9862
Fe-0.1Cu1.29235.3291
Fe-0.3Cu1.76247.8542
Fe-0.5Cu2.01452.8991
表5  650 K下演化50步后不同Fe-Cu合金的临界团簇半径与平均浓度计算结果
图9  650 K下演化50步后不同Fe-Cu合金临界团簇中Cu元素浓度的一维分布曲线
图10  不同温度和不同Cu元素浓度下演化50步后团簇半径的变化曲线
图11  650 K下演化50步后不同辐照强度下Fe-0.3%Cu和Fe-0.5%Cu合金临界团簇状态的空位增量分布图
图12  650 K下演化50步后辐照强度0.01 dpa/s下Fe-0.3%Cu合金在不同时刻的空位浓度分布
t / stepRC / nmMin.CVMax.CV - Min.CVSum.CV
301.5580.001028.63 × 10-517.149
601.7630.001823.89 × 10-434.381
901.8840.002298.92 × 10-451.535
1202.0390.002801.65 × 10-369.190
表6  演化50步后不同时刻下团簇空位浓度信息计算结果
1 Li Z C, Chen L. Irradiation embrittlement mechanisms and relevant influence factors of nuclear reactor pressure vessel steels [J]. Acta Metall. Sin., 2014, 50: 1285
1 李正操, 陈 良. 核能系统压力容器辐照脆化机制及其影响因素 [J]. 金属学报, 2014, 50: 1285
doi: 10.11900/0412.1961.2014.00189
2 Klueh R L, Harries D R. High-Chromium Ferritic and Martensitic Steels for Nuclear Applications [M]. West Conshohocken, PA: ASTM, 2001: 1
3 Grobner P J. The 885°F (475oC) embrittlement of ferritic stainless steels [J]. Metall. Trans., 1973, 4: 251
4 Sharma T, Bonagani S K, Kumar N N, et al. Detection of intergranular embrittlement of reactor pressure vessel steel by electrochemical method [J]. Mater. Sci. Eng., 2018, A725: 88
5 Bergner F, Gillemot F, Hernández-Mayoral M, et al. Contributions of Cu-rich clusters, dislocation loops and nanovoids to the irradiation-induced hardening of Cu-bearing low-Ni reactor pressure vessel steels [J]. J. Nucl. Mater., 2015, 461: 37
doi: 10.1016/j.jnucmat.2015.02.031
6 Lambrecht M, Malerba L, Almazouzi A. Influence of different chemical elements on irradiation-induced hardening embrittlement of RPV steels [J]. J. Nucl. Mater., 2008, 378: 282
doi: 10.1016/j.jnucmat.2008.06.030
7 Hernández-Mayoral M, Gómez-Briceño D. Transmission electron microscopy study on neutron irradiated pure iron and RPV model alloys [J]. J. Nucl. Mater., 2010, 399: 146
doi: 10.1016/j.jnucmat.2009.11.013
8 Ke H B, Wells P, Edmondson P D, et al. Thermodynamic and kinetic modeling of Mn-Ni-Si precipitates in low-Cu reactor pressure vessel steels [J]. Acta Mater., 2017, 138: 10
doi: 10.1016/j.actamat.2017.07.021
9 Sun Z Y, Yang C, Liu W B. Phase field simulations of the sintering process of UO2 [J]. Acta Metall. Sin., 2020, 56: 1295
9 孙正阳, 杨 超, 柳文波. UO2烧结过程的相场模拟 [J]. 金属学报, 2020, 56: 1295
doi: 10.11900/0412.1961.2019.00440
10 Kundin J, Sohaib H, Schiedung R, et al. Phase-field modeling of pores and precipitates in polycrystalline system [J]. Model. Simul. Mater. Sci. Eng., 2018, 26: 065003
11 Hötzer J, Seiz M, Kellner M, et al. Phase-field simulation of solid state sintering [J]. Acta Mater., 2019, 164: 184
doi: 10.1016/j.actamat.2018.10.021
12 Fan D, Chen L Q. Computer simulation of grain growth using a continuum field model [J]. Acta Mater., 1997, 45: 611
doi: 10.1016/S1359-6454(96)00200-5
13 Yin B Y. Ceramic Nuclear Fuel Process [M]. Harbin: Harbin Engineering University Press, 2016: 277
13 尹邦跃. 陶瓷核燃料工艺 [M]. 哈尔滨: 哈尔滨工程大学出版社, 2016: 277
14 Molnar D, Mukherjee R, Choudhury A, et al. Multiscale simulations on the coarsening of Cu-rich precipitates in α-Fe using kinetic Monte Carlo, molecular dynamics and phase-field simulations [J]. Acta Mater., 2012, 60: 6961
doi: 10.1016/j.actamat.2012.08.051
15 Zhu J M, Zhang T L, Yang Y, et al. Phase field study of the copper precipitation in Fe-Cu alloy [J]. Acta Mater., 2019, 166: 560
doi: 10.1016/j.actamat.2019.01.009
16 Zhao B J, Zhao Y H, Sun Y Y, et al. Effect of Mn composition on the nanometer Cu-rich phase of Fe-Cu-Mn alloy by phase field method [J]. Acta Metall. Sin., 2019, 55: 593
16 赵宝军, 赵宇宏, 孙远洋 等. Mn含量对Fe-Cu-Mn合金纳米富Cu析出相影响的相场法研究 [J]. 金属学报, 2019, 55: 593
doi: 10.11900/0412.1961.2018.00506
17 Yan Z W, Shi S J, Li Y S, et al. Vacancy and interstitial atom evolution with the separation of the nanoscale phase in Fe-Cr alloys: Phase-field simulations [J]. Phys. Chem. Chem. Phys., 2020, 22: 3611
doi: 10.1039/C9CP06247E
18 Li B Y, Hu S Y, Li C L, et al. Simulations of irradiated-enhanced segregation and phase separation in Fe-Cu-Mn alloys [J]. Model. Simul. Mater. Sci. Eng., 2017, 25: 065007
19 Weinan E, Ren W Q, Vanden-Eijnden E. Simplified and improved string method for computing the minimum energy paths in barrier-crossing events [J]. J. Chem. Phys., 2007, 126: 164103
doi: 10.1063/1.2720838
20 Maragliano L, Fischer A, Vanden-Eijnden E, et al. String method in collective variables: Minimum free energy paths and isocommittor surfaces [J]. J. Chem. Phys., 2006, 125: 024106
21 Li B Y. Modelling and simulation in radiation induced defects in reactor pressure vessel steels [D]. Beijing: Tsinghua University, 2018
21 李博岩. 反应堆压力容器钢辐照损伤的计算模拟研究 [D]. 北京: 清华大学, 2018
22 Li B Y, Zhang L, Li C L, et al. Finding Non-classical critical nuclei and minimum energy path of Cu precipitates in Fe-Cu alloys [J]. Model. Simul. Mater. Sci. Eng., 2017, 25: 085006
23 Zhang L, Chen L Q, Du Q. Mathematical and numerical aspects of a phase-field approach to critical nuclei morphology in solids [J]. J. Sci. Comput., 2008, 37: 89
doi: 10.1007/s10915-008-9207-7
24 Zhang L, Chen L Q, Du Q. Diffuse-interface approach to predicting morphologies of critical nucleus and equilibrium structure for cubic to tetragonal transformations [J]. J. Comput. Phys., 2010, 229: 6574
doi: 10.1016/j.jcp.2010.05.013
25 Chen L Q, Shen J. Applications of semi-implicit Fourier-spectral method to phase field equations [J]. Comput. Phys. Commun., 1998, 108: 147
doi: 10.1016/S0010-4655(97)00115-X
26 Wang Y U. Computer modeling and simulation of solid-state sintering: A phase field approach [J]. Acta Mater., 2006, 54: 953
doi: 10.1016/j.actamat.2005.10.032
27 Cahn J W, Hilliard J E. Free energy of a nonuniform system. III. Nucleation in a two-component incompressible fluid [J]. J. Chem. Phys., 1959, 31: 688
doi: 10.1063/1.1730447
28 Biner S B. Programming Phase-Field Modeling [M]. Cham: Springer, 2017: 1
29 Hu S Y, Chen L Q. A phase-field model for evolving microstructures with strong elastic inhomogeneity [J]. Acta Mater., 2001, 49: 1879
doi: 10.1016/S1359-6454(01)00118-5
30 Peng H J, Xie Y Q, Liu S Q. Research on atomic states, physical properties and catalytic performance of Ru metal [J]. Sci. China, 2007, 50E: 177
31 Breeman M, Boerma D O. Migration of Cu adatoms on a Cu(100) surface, studied with low-energy ion scattering (LEIS) [J]. Surf. Sci., 1992, 269-270: 224
doi: 10.1016/0039-6028(92)91254-9
32 Cahn J W. On spinodal decomposition [J]. Acta Metall., 1961, 9: 795
doi: 10.1016/0001-6160(61)90182-1
33 Ke J H, Reese E R, Marquis E A, et al. Flux effects in precipitation under irradiation—Simulation of Fe-Cr alloys [J]. Acta Mater., 2018, 164: 586
doi: 10.1016/j.actamat.2018.10.063
34 Makin M J, Minter F J. Irradiation hardening in copper and nickel [J]. Acta Metall., 1960, 8: 691
doi: 10.1016/0001-6160(60)90200-5
35 Odette G R, Yamamoto T, Klingensmith D. On the effect of dose rate on irradiation hardening of RPV steels [J]. Philos. Mag., 2005, 85: 779
doi: 10.1080/14786430412331319910
36 Mohapatra J N, Kamada Y, Kikuchi H, et al. Effect of Cr-rich phase precipitation on magnetic and mechanical properties of Fe-20% Cr alloy [J]. IEEE Trans. Magn., 2011, 47: 4356
doi: 10.1109/TMAG.2011.2155047
37 Nagano T, Enomoto M. Simulation of the growth of copper critical nucleus in dilute bcc Fe-Cu alloys [J]. Scr. Mater., 2006, 55: 223
doi: 10.1016/j.scriptamat.2006.04.015
38 Garcke H, Kwak D J C. On asymptotic limits of Cahn-Hilliard systems with elastic misfit [A]. Analysis, Modeling and Simulation of Multiscale Problems [M]. Berlin Heidelberg: Springer, 2006: 87
39 Koyama T, Onodera H. Computer simulation of phase decomposition in Fe-Cu-Mn-Ni quaternary alloy based on the phase-field method [J]. Metall. Trans., 2005, 46: 1187
40 Li Y L, Hu S Y, Zhang L, et al. Non-classical nuclei and growth kinetics of Cr precipitates in FeCr alloys during ageing [J]. Model. Simul. Mater. Sci. Eng., 2014, 22: 025002
41 Zhang C, Enomoto M, Yamashita T, et al. Cu precipitation in a prestrained Fe-1.5 wt pct Cu alloy during isothermal aging [J]. Metall. Mater. Trans., 2004, 35A: 1263
42 Saridakis E. Optimization of the critical nuclear size for protein crystallization: A note [J]. Acta Cryst., 2000, D56: 106
[1] 朱小绘, 刘向兵, 王润中, 李远飞, 刘文庆. 290℃氩离子辐照对Fe-Cu合金微观组织的影响[J]. 金属学报, 2022, 58(7): 905-910.
[2] 赵彦,张洪宇,韦华,郑启,金涛,孙晓峰. 相场法研究含第二相颗粒多晶体系的晶粒粗化标度律[J]. 金属学报, 2013, 49(8): 981-988.
[3] 周广钊 王永欣 陈铮. 相场法模拟不同形状的硬质颗粒对两相晶粒长大的影响[J]. 金属学报, 2012, 48(2): 227-234.
[4] 贺新福 杨鹏 杨文. Fe-Cu合金基体损伤的分子动力学模拟研究[J]. 金属学报, 2011, 47(7): 954-957.
[5] 张玉妥; 庞维诚 . 用相场方法模拟纯物质等轴枝晶生长[J]. 金属学报, 2000, 36(6): 589-591 .
[6] 许裕生;江焕宏;钱敏;金宗明;王耀荣;仇国阳;马荣兵;薛青. 少量硼对Fe-Cu纳米粉粒固溶度的影响[J]. 金属学报, 1997, 33(8): 807-813.