| 单晶高温合金近服役环境下的变形损伤行为 |
张健( ), 王栋( ), 李亚微, 黄亚奇, 展鑫, 谢光 |
| 中国科学院金属研究所 沈阳 110016 |
|
| Deformation and Damage Behavior of Single Crystal Superalloys Under Near-Service Conditions |
ZHANG Jian( ), WANG Dong( ), LI Yawei, HUANG Yaqi, ZHAN Xin, XIE Guang |
| Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China |
引用本文:
张健, 王栋, 李亚微, 黄亚奇, 展鑫, 谢光. 单晶高温合金近服役环境下的变形损伤行为[J]. 金属学报, 2026, 62(5): 875-889.
Jian ZHANG,
Dong WANG,
Yawei LI,
Yaqi HUANG,
Xin ZHAN,
Guang XIE.
Deformation and Damage Behavior of Single Crystal Superalloys Under Near-Service Conditions[J]. Acta Metall Sin, 2026, 62(5): 875-889.
| [1] |
Zhang J, Wang L, Xie G, et al. Recent progress in research and development of nickel-based single crystal superalloys [J]. Acta Metall. Sin., 2023, 59: 1109
doi: 10.11900/0412.1961.2023.00140
|
| [1] |
张 健, 王 莉, 谢 光 等. 镍基单晶高温合金的研发进展 [J]. 金属学报, 2023, 59: 1109
|
| [2] |
Li Y W. Study on high temperature creep and very high cycle fatigue behaviors of a 3rd generation Ni-based single crystal superalloy [D]. Hefei: University of Science and Technology of China, 2023
|
| [2] |
李亚微. 一种第三代镍基单晶高温合金高温蠕变与超高周疲劳行为研究 [D]. 合肥: 中国科学技术大学, 2023
|
| [3] |
He Y F, Wang S G, Shen J, et al. Evolution of micro-pores in a single crystal nickel-based superalloy during 980 oC creep [J]. Acta Metall. Sin. (Engl. Lett.), 2022, 35: 1397
doi: 10.1007/s40195-021-01371-6
|
| [4] |
Yu Z Y, Wang X M, Liang H, et al. Thickness debit effect in Ni-based single crystal superalloys at different stress levels [J]. Int. J. Mech. Sci., 2020, 170: 105357
doi: 10.1016/j.ijmecsci.2019.105357
|
| [5] |
Zhang Y, Xu R D, Hu J K, et al. A thickness debit effect characterization parameter for creep rupture behaviors of nickel-based single crystal superalloys [J]. J. Mater. Res. Technol., 2024, 29: 3522
doi: 10.1016/j.jmrt.2024.01.238
|
| [6] |
Seetharaman V, Cetel A D. Thickness debit in creep properties of PWA 1484 [A]. Superalloys 2004 [M]. Warrendale, PA: TMS, 2004: 207
|
| [7] |
Zhang S Q, Ma G Q, Wang H B, et al. Thickness debit effect in creep performance of a Ni3Al-based single-crystal superalloy with [001] orientation [J]. Crystals, 2023, 13: 200
doi: 10.3390/cryst13020200
|
| [8] |
Wu J J, Meng J, Zou M K, et al. Effect of wall thickness on micropores and stress-rupture properties of a single-crystal nickel-based superalloy [J]. Mater. Sci. Eng., 2023, A872: 144941
|
| [9] |
Lv J J, Zhao Y S, Wang S, et al. Stress state mechanism of thickness debit effect in creep performances of a Ni-based single crystal superalloy [J]. Int. J. Plast., 2022, 159: 103470
doi: 10.1016/j.ijplas.2022.103470
|
| [10] |
Liu J, Yu M H, Min S L, et al. The effect of secondary dendrite orientation on thickness debit effect of nickel-based single-crystal superalloy with tubular samples [J]. J. Mater. Sci. Technol., 2025, 217: 80
doi: 10.1016/j.jmst.2024.06.056
|
| [11] |
Li Y F. Anisotropic creep properties of a 3rd generation nickel-base single crystal superalloy [D]. Hefei: University of Science and Technology of China, 2019
|
| [11] |
李一飞. 一种第三代镍基单晶高温合金蠕变各向异性的研究 [D]. 合肥: 中国科学技术大学, 2019
|
| [12] |
Xiao Q F, Xu Y M, Liu X L, et al. Oxidation-induced recrystallization and damage mechanism of a Ni-based single-crystal superalloy during creep [J]. Mater. Charact., 2023, 195: 112465
doi: 10.1016/j.matchar.2022.112465
|
| [13] |
Yang B S, Li B, Zhang Y N. Creep rupture of smoothed and notched DD6 single crystal superalloy specimens subjected to high-temperature hot corrosion [J]. Mater. Des., 2025, 249: 113526
doi: 10.1016/j.matdes.2024.113526
|
| [14] |
Yang Y Q, Zhao Y C, Wen Z X, et al. Study on the hot corrosion-creep failure mechanism of Ni-based single crystal superalloy considering the stress dependence [J]. Mater. Sci. Eng., 2024, A897: 146350
|
| [15] |
Liu H, Wang X M, Zhao Z N, et al. The analysis on creep failure mechanism of nickel-based single crystal superalloys deposited with different molten salts [J]. Eng. Failure Anal., 2023, 147: 107171
doi: 10.1016/j.engfailanal.2023.107171
|
| [16] |
Liu H, Wang X M, Liu P Y, et al. Experimental and chemo-mechanical analysis of hot corrosion influence on creep properties of DD6 single crystal superalloy in molten NaCl salt [J]. Eng. Fract. Mech., 2022, 260: 108194
doi: 10.1016/j.engfracmech.2021.108194
|
| [17] |
Caccuri V, Cormier J, Desmorat R. γ′-rafting mechanisms under com-plex mechanical stress state in Ni-based single crystalline superalloys [J]. Mater. Des., 2017, 131: 487
doi: 10.1016/j.matdes.2017.06.018
|
| [18] |
Cao L, Wollgramm P, Bürger D, et al. How evolving multiaxial stress states affect the kinetics of rafting during creep of single crystal Ni-base superalloys [J]. Acta Mater., 2018, 158: 381
doi: 10.1016/j.actamat.2018.07.061
|
| [19] |
Yang B S, Li B. Creep notch effect in DD6 Ni-based single crystal superalloy: Experimental and modeling studies [J]. Mater. Sci. Eng., 2025, A931: 148221
|
| [20] |
Huang J, Qin H J, Li R H, et al. Influence of loading sequence on notch creep behavior of Ni-based single crystal superalloy [J]. Mater. Sci. Eng., 2025, A939: 148472
|
| [21] |
Bao P Y, Wang J W, Zhao H G, et al. Creep behavior and mechanism of a notched γ′-rich Ni-based single crystal superalloy at high temperature [J]. Mater. Sci. Eng., 2025, A925: 147883
|
| [22] |
Qi D Q, Wang L, Zhao P, et al. Facilitating effect of interfacial grooves on the rafting of nickel-based single crystal superalloy at high temperature [J]. Scr. Mater., 2019, 167: 71
doi: 10.1016/j.scriptamat.2019.04.001
|
| [23] |
Kontis P, Li Z M, Collins D M, et al. The effect of chromium and cobalt segregation at dislocations on nickel-based superalloys [J]. Scr. Mater., 2018, 145: 76
doi: 10.1016/j.scriptamat.2017.10.005
|
| [24] |
Ru Y, Li S S, Zhou J, et al. Dislocation network with pair-coupling structure in {111} γ/γ′ interface of Ni-based single crystal superalloy [J]. Sci. Rep., 2016, 6: 29941
doi: 10.1038/srep29941
|
| [25] |
Li Y W, Wang L, He Y F, et al. Role of interfacial dislocation networks during secondary creep at elevated temperatures in a single crystal Ni-based superalloy [J]. Scr. Mater., 2022, 217: 114769
doi: 10.1016/j.scriptamat.2022.114769
|
| [26] |
Li Y W, Wang L, Lou L H, et al. Stress effect on rupture mechanisms of a third generation single crystal superalloy crept at ultra-high temperature [J]. Aeronaut. Manuf. Technol., 2023, 66(4): 48
|
| [26] |
李亚微, 王 莉, 楼琅洪 等. 应力对第3代单晶高温合金超高温蠕变断裂机制的影响 [J]. 航空制造技术, 2023, 66(4): 48
|
| [27] |
Gao Y H, Ru Y, Zhao W Y, et al. Exceptional ultra-high temperature creep resistance of a [111]-oriented single crystal superalloy [J]. Scr. Mater., 2024, 246: 116093
doi: 10.1016/j.scriptamat.2024.116093
|
| [28] |
Tian N, Zhao G Q, Shi Z Z, et al. High-temperature creep behaviour and deformation mechanism of a high-concentration Re/Ru single-crystal nickel-based alloy [J]. J. Mater. Res. Technol., 2024, 29: 1350
doi: 10.1016/j.jmrt.2024.01.131
|
| [29] |
Luo L, Ru Y, Ma Y, et al. Design for 1200 oC creep properties of Ni-based single crystal superalloys: Effect of γ′-forming elements and its microscopic mechanism [J]. Mater. Sci. Eng., 2022, A832: 142494
|
| [30] |
Lukáš P, Čadek J, Kunz L, et al. Creep resistance of single crystal superalloys CMSX-4 and CM186LC [J]. Kovove Mater., 2005, 43: 5
|
| [31] |
Lu F, Lu S, Antonov S, et al. Duration-affected creep behaviors of Ni-based single crystal superalloys with/without rhenium addition designed for IGT application [J]. Mater. Sci. Eng., 2023, A864: 144560
|
| [32] |
Dubiel B, Czyrska-Filemonowicz A. TEM analyses of microstructure evolution in ex-service single crystal CMSX-4 gas turbine blade [J]. Solid State Phenom., 2012, 186: 139
doi: 10.4028/www.scientific.net/SSP.186
|
| [33] |
Giraud R, Hervier Z, Cormier J, et al. Strain effect on the γ′ dissolution at high temperatures of a nickel-based single crystal superalloy [J]. Metall. Mater. Trans., 2013, 44A: 131
|
| [34] |
Cormier J, Milhet X, Mendez J. Non-isothermal creep at very high temperature of the nickel-based single crystal superalloy MC2 [J]. Acta Mater., 2007, 55: 6250
doi: 10.1016/j.actamat.2007.07.048
|
| [35] |
Le Graverend J B, Dirand L, Jacques A, et al. In situ measurement of the γ/γ′ lattice mismatch evolution of a nickel-based single-crystal superalloy during non-isothermal very high-temperature creep experiments [J]. Metall. Mater. Trans., 2012, 43A: 3946
|
| [36] |
le Graverend J B, Cormier J, Jouiad M, et al. Effect of fine γ′ precipitation on non-isothermal creep and creep-fatigue behaviour of nickel base superalloy MC2 [J]. Mater. Sci. Eng., 2010, A527: 5295
|
| [37] |
Cormier J. Thermal cycling creep resistance of Ni-based single crystal superalloys [A]. Superalloys 2016: Proceedings of the 13th International Symposium of Superalloys [M]. Warrendale, PA: TMS, 2016: 385
|
| [38] |
Milhet X, Cormier J, Organista A. On the role of the internal stress during non-isothermal creep life of a first generation nickel based single crystal superalloy [J]. Mater. Sci. Eng., 2010, A527: 2280
|
| [39] |
Ge C T, Liu L R, Lv P S, et al. Microstructure and stress rupture properties degradation of a 2nd generation single crystal superalloy during short-duration overheating [J]. Mater. Today Commun., 2025, 44: 111960
|
| [40] |
Schwalbe C, Cormier J, Jones C N, et al. Investigating the dislocation-driven micro-mechanical response under non-isothermal creep conditions in single-crystal superalloys [J]. Metall. Mater. Trans., 2018, 49A: 3988
|
| [41] |
Duan H D, Kang J, Li G, et al. Effects of ultra-high-temperature thermal cycles on the microstructure evolution and creep behavior of a high γ′ volume fraction nickel-based single-crystal superalloy [J]. J. Alloys Compd., 2025, 1035: 181590
doi: 10.1016/j.jallcom.2025.181590
|
| [42] |
Liang J W. The creep properties of nickel-based single crystal superalloy under overheating and overload conditions [D]. Xi’an: Northwestern Polytechnical University, 2018
|
| [42] |
梁建伟. 镍基单晶合金超温超载蠕变性能研究 [D]. 西安: 西北工业大学, 2018
|
| [43] |
Hantcherli M, Pettinari-Sturmel F, Viguier B, et al. Evolution of interfacial dislocation network during anisothermal high-temperature creep of a nickel-based superalloy [J]. Scr. Mater., 2012, 66: 143
doi: 10.1016/j.scriptamat.2011.10.022
|
| [44] |
Viguier B, Touratier F, Andrieu E. High-temperature creep of single-crystal nickel-based superalloy: Microstructural changes and effects of thermal cycling [J]. Philos. Mag., 2011, 91: 4427
doi: 10.1080/14786435.2011.609151
|
| [45] |
Zhang J, Wang L, Wang D, et al. Recent progress in research and development of nickel-based single crystal superalloys [J]. Acta Metall. Sin., 2019, 55: 1077
|
| [45] |
张 健, 王 莉, 王 栋 等. 镍基单晶高温合金的研发进展 [J]. 金属学报, 2019, 55: 1077
|
| [46] |
Cowles B A. High cycle fatigue in aircraft gas turbines—An industry perspective [J]. Int. J. Fract., 1996, 80: 147
doi: 10.1007/BF00012667
|
| [47] |
Beardmore P, Davies R G, Johnston T L. On the temperature dependence of the flow stress of nickel-base alloys [J]. Trans. Metall. Soc. AIME, 1969, 245: 1537
|
| [48] |
Xu J C, Zhao X B, Chen J S, et al. Temperature-dependent microscopic deformation mechanisms and performance enhancement prospects in high-cycle fatigue of nickel-based single crystal superalloys [J]. Int. J. Plast., 2025, 184: 104207
doi: 10.1016/j.ijplas.2024.104207
|
| [49] |
He Z W, Zhang Y Y, Qiu W H, et al. Temperature effect on the low cycle fatigue behavior of a directionally solidified nickel-base superalloy [J]. Mater. Sci. Eng., 2016, A676: 246
|
| [50] |
Li P, Li Q Q, Jin T, et al. Comparison of low-cycle fatigue behaviors between two nickel-based single-crystal superalloys [J]. Int. J. Fatigue, 2014, 63: 137
doi: 10.1016/j.ijfatigue.2014.01.018
|
| [51] |
Zhang L, Zhao L G, Roy A, et al. Low-cycle fatigue of single crystal nickel-based superalloy—Mechanical testing and TEM characterisation [J]. Mater. Sci. Eng., 2019, A744: 538
|
| [52] |
Fan Y S, Yang X G, Tan L, et al. Experiment and modelling on the effect of microstructural morphology on fatigue life of a Ni-based superalloy [J]. Mater. Sci. Eng., 2020, A786: 139368
|
| [53] |
Ma X F, Shi H J. In situ SEM studies of the low cycle fatigue behavior of DZ4 superalloy at elevated temperature: Effect of partial recrystallization [J]. Int. J. Fatigue, 2014, 61: 255
doi: 10.1016/j.ijfatigue.2013.11.001
|
| [54] |
Rémy L, Geuffrard M, Alam A, et al. Effects of microstructure in high temperature fatigue: Lifetime to crack initiation of a single crystal superalloy in high temperature low cycle fatigue [J]. Int. J. Fatigue, 2013, 57: 37
doi: 10.1016/j.ijfatigue.2012.10.013
|
| [55] |
Morrissey R J, John R, Porter III W J. Fatigue variability of a single crystal superalloy at elevated temperature [J]. Int. J. Fatigue, 2009, 31: 1758
doi: 10.1016/j.ijfatigue.2009.03.013
|
| [56] |
Prasad K, Sarkar R, Gopinath K. Role of shrinkage pores, carbides on cyclic deformation behaviour of conventionally cast nickel base superalloy CM247LC® at 870 oC [J]. Mater. Sci. Eng., 2016, A654: 381
|
| [57] |
Reuchet J, Remy L. Fatigue oxidation interaction in a superalloy—Application to life prediction in high temperature low cycle fatigue [J]. Metall. Trans., 1983, 14A: 141
|
| [58] |
Ma X F, Shi H J, Gu J L. In-situ scanning electron microscopy studies of small fatigue crack growth in recrystallized layer of a directionally solidified superalloy [J]. Mater. Lett., 2010, 64: 2080
doi: 10.1016/j.matlet.2010.06.044
|
| [59] |
Zhang L, Zhao L G, Roy A, et al. In-situ SEM study of slip-controlled short-crack growth in single-crystal nickel superalloy [J]. Mater. Sci. Eng., 2019, A742: 564
|
| [60] |
Lamm M, Singer R F. The effect of casting conditions on the high-cycle fatigue properties of the single-crystal nickel-base superalloy PWA 1483 [J]. Metall. Mater. Trans., 2007, 38A: 1177
|
| [61] |
Bortoluci Ormastroni L M, Mataveli Suave L, Cervellon A, et al. LCF, HCF and VHCF life sensitivity to solution heat treatment of a third-generation Ni-based single crystal superalloy [J]. Int. J. Fatigue, 2020, 130: 105247
doi: 10.1016/j.ijfatigue.2019.105247
|
| [62] |
Fritzemeier L G. The influence of high thermal gradient casting, hot isostatic pressing and alternate heat treatment on the structure and properties of a single crystal nickel base superalloy [A]. Superalloys 1988 [M]. Warrendale, PA: TMS, 1988: 265
|
| [63] |
Steuer S, Villechaise P, Pollock T M, et al. Benefits of high gradient solidification for creep and low cycle fatigue of AM1 single crystal superalloy [J]. Mater. Sci. Eng., 2015, A645: 109
|
| [64] |
Huang Y Q, Wang D, Shen J, et al. Initiation of fatigue cracks in a single-crystal nickel-based superalloy at intermediate temperature [A]. Superalloys 2020: Proceedings of the 14th International Symposium on Superalloys [M]. Cham: Springer, 2020: 208
|
| [65] |
Huang Y Q, Wang D, Lu Y Z, et al. Fatigue crack initiation behavior at intermediate temperature under high stress amplitude for single crystal superalloy DD413 [J]. Chin. J. Mater. Res., 2021, 35: 510
doi: 10.11901/1005.3093.2020.274
|
| [65] |
黄亚奇, 王 栋, 卢玉章 等. 第一代单晶高温合金中温高应力幅下的疲劳裂纹萌生行为 [J]. 材料研究学报, 2021, 35: 510
doi: 10.11901/1005.3093.2020.274
|
| [66] |
Ruttert B, Meid C, Roncery L M, et al. Effect of porosity and eutectics on the high-temperature low-cycle fatigue performance of a nickel-base single-crystal superalloy [J]. Scr. Mater., 2018, 155: 139
doi: 10.1016/j.scriptamat.2018.06.036
|
| [67] |
Liu Y H, Kang M D, Wu Y, et al. Effects of microporosity and precipitates on the cracking behavior in polycrystalline superalloy Inconel 718 [J]. Mater. Charact., 2017, 132: 175
doi: 10.1016/j.matchar.2017.08.012
|
| [68] |
Kontis P, Alabort E, Barba D, et al. On the role of boron on improving ductility in a new polycrystalline superalloy [J]. Acta Mater., 2017, 124: 489
doi: 10.1016/j.actamat.2016.11.009
|
| [69] |
Kontis P, Yusof H A M, Pedrazzini S, et al. On the effect of boron on grain boundary character in a new polycrystalline superalloy [J]. Acta Mater., 2016, 103: 688
doi: 10.1016/j.actamat.2015.10.006
|
| [70] |
Lukáš P, Kunz L. Cyclic slip localisation and fatigue crack initiation in fcc single crystals [J]. Mater. Sci. Eng., 2001, A314: 75
|
| [71] |
Lukáš P, Kunz L. Role of persistent slip bands in fatigue [J]. Philos. Mag., 2004, 84: 317
doi: 10.1080/14786430310001610339
|
| [72] |
Brundidge C L, Pollock T M. Processing to fatigue properties: Benefits of high gradient casting for single crystal airfoils [A]. Superalloys 2012 [C]. Hoboken: Wiley, 2012: 379
|
| [73] |
Huang Y Q, Wang S G, Lu Y Z, et al. Ex-situ investigation of micro-pore evolution and crack initiation/propagation during fatigue in a single crystal Ni-based superalloy [J]. Mater. Sci. Eng., 2025, A947: 149224
|
| [74] |
Furuya Y, Kobayashi K, Hayakawa M, et al. High-temperature ultrasonic fatigue testing of single-crystal superalloys [J]. Mater. Lett., 2012, 69: 1
doi: 10.1016/j.matlet.2011.11.066
|
| [75] |
Cervellon A, Hémery S, Kürnsteiner P, et al. Crack initiation mechanisms during very high cycle fatigue of Ni-based single crystal superalloys at high temperature [J]. Acta Mater., 2020, 188: 131
doi: 10.1016/j.actamat.2020.02.012
|
| [76] |
Very high cycle fatigue at elevated temperatures: A review on high temperature ultrasonic fatigue [J]. J. Space Saf. Eng., 2022, 9: 488
|
| [77] |
Ranc N, Wagner D, Paris P C. Study of thermal effects associated with crack propagation during very high cycle fatigue tests [J]. Acta Mater., 2008, 56: 4012
doi: 10.1016/j.actamat.2008.04.023
|
| [78] |
Zhao Z, Zhang F, Dong C, et al. Initiation and early-stage growth of internal fatigue cracking under very-high-cycle fatigue regime at high temperature [J]. Metall. Mater. Trans., 2020, 51A: 1575
|
| [79] |
Morales A V, Mauget F, Larrouy B, et al. Very high cycle fatigue of a notched Ni-based single crystal superalloy at high temperature [J]. Int. J. Fatigue, 2024, 186: 108379
doi: 10.1016/j.ijfatigue.2024.108379
|
| [80] |
Cervellon A, Cormier J, Mauget F, et al. Very high cycle fatigue of Ni-based single-crystal superalloys at high temperature [J]. Metall. Mater. Trans., 2018, 49A: 3938
|
| [81] |
Cervellon A, Ormastroni L M B, Hervier Z, et al. Damage mechanisms during very high cycle fatigue of a coated and grit-blasted Ni-based single-crystal superalloy [J]. Int. J. Fatigue, 2021, 142: 105962
doi: 10.1016/j.ijfatigue.2020.105962
|
| [82] |
Li Y W, Wang D, He Y F, et al. High temperature VHCF of a 3rd generation Ni-based single crystal superalloy with different casting pore sizes [J]. Int. J. Fatigue, 2023, 175: 107804
doi: 10.1016/j.ijfatigue.2023.107804
|
| [83] |
Zhao Z, Li Q, Zhang F, et al. Transition from internal to surface crack initiation of a single-crystal superalloy in the very-high-cycle fatigue regime at 1100 oC [J]. Int. J. Fatigue, 2021, 150: 106343
doi: 10.1016/j.ijfatigue.2021.106343
|
| [84] |
Zhou Z F, Wang D K, Li R G, et al. Quantifying the impact of oxidized carbide expansion on fatigue crack initiation in a Ni-based single-crystal superalloy [J]. Mater. Charact., 2025, 220: 114701
doi: 10.1016/j.matchar.2024.114701
|
| [85] |
Yi W J, Huang Y Q, Wang S G, et al. Quasi in-situ investigation of very high cycle fatigue in a third generation nickel-based single crystal superalloy at high temperature [A]. Chinese Materials Conference 2025 [C]. Xia'men: Chinese Materials Research Society, 2025
|
| [85] |
易文静, 黄亚奇, 王绍钢 等. 第三代镍基单晶高温合金高温超高周疲劳准原位研究 [A]. 中国材料大会2025 [C]. 厦门: 中国材料研究学会, 2025
|
| [86] |
Lu P, Jin X C, Li P, et al. Crystal plasticity constitutive model and thermodynamics informed creep-fatigue life prediction model for Ni-based single crystal superalloy [J]. Int. J. Fatigue, 2023, 176: 107829
doi: 10.1016/j.ijfatigue.2023.107829
|
| [87] |
Yin Q, Wang J D, Wen Z X, et al. Creep-fatigue behavior of nickel-based single crystal superalloy with different orientations: Experimental characterization and multi-scale simulation [J]. Mater. Sci. Eng., 2023, A886: 145667
|
| [88] |
Song J N, Li Z L, Tan H J, et al. A comparative study of creep-fatigue life prediction for complex geometrical specimens using supervised machine learning [J]. Eng. Fract. Mech., 2023, 291: 109567
doi: 10.1016/j.engfracmech.2023.109567
|
| [89] |
Xu J W, Luo C, Li J Z, et al. Multiscale modeling of oxidation-fatigue damage mechanisms under compressive dwell-fatigue loading conditions for nickel-based single-crystal superalloy [J]. Eng. Fract. Mech., 2025, 315: 110823
doi: 10.1016/j.engfracmech.2025.110823
|
| [90] |
Meng Y, Zhou C G, Zhao Z H, et al. Effect of oxidation on the competition between internal and external fatigue crack initiation of Ni-based single crystal superalloy [J]. Int. J. Fatigue, 2025, 197: 108930
doi: 10.1016/j.ijfatigue.2025.108930
|
| [91] |
Martin A, Drouelle E, Rame J, et al. Low cycle fatigue/corrosion interactions at 950 oC of AM1 single crystal nickel-based superalloy [J]. High Temp. Corros. Mater., 2024, 101: 961
|
| [92] |
Shrestha R, Simsiriwong J, Shamsaei N. Fatigue behavior of additive manufactured 316L stainless steel under axial versus rotating-bending loading: Synergistic effects of stress gradient, surface roughness, and volumetric defects [J]. Int. J. Fatigue, 2021, 144: 106063
doi: 10.1016/j.ijfatigue.2020.106063
|
| [93] |
Beevers E, Brandão A D, Gumpinger J, et al. Fatigue properties and material characteristics of additively manufactured AlSi10Mg—Effect of the contour parameter on the microstructure, density, residual stress, roughness and mechanical properties [J]. Int. J. Fatigue, 2018, 117: 148
doi: 10.1016/j.ijfatigue.2018.08.023
|
| [94] |
Yu J J, Yang Y H, Sun X F, et al. Rotary bending high-cycle fatigue behavior of DD32 single crystal superalloy containing rhenium [J]. J. Mater. Sci., 2012, 47: 4805
doi: 10.1007/s10853-012-6323-4
|
| [95] |
Liu L Y, Gao X Y, Yang X F, et al. Vibration fatigue properties and fracture mechanism of DD6 single crystal superalloy [J]. J. Mater. Eng., 2018, 46(2): 128
doi: 10.11868/j.issn.1001-4381.2016.000891
|
| [95] |
刘丽玉, 高翔宇, 杨宪锋 等. DD6单晶高温合金振动疲劳性能及断裂机理 [J]. 材料工程, 2018, 46(2): 128
doi: 10.11868/j.issn.1001-4381.2016.000891
|
| [96] |
Lu H, Wang J D, Lian Y D, et al. Effect of orientation deviation on random vibration fatigue behavior of nickel based single crystal superalloy [J]. Int. J. Fatigue, 2023, 177: 107930
doi: 10.1016/j.ijfatigue.2023.107930
|
| [97] |
Xu W, Zhu B C, Chen X, et al. Thickness debit effect of Ni-based single crystal superalloy thin-walled specimens in the VHCF regime based on a vibration fatigue test [J]. J. Mater. Res. Technol., 2024, 33: 2538
doi: 10.1016/j.jmrt.2024.09.247
|
| [98] |
Zhao Y J, Song Y Y, Yang W Z, et al. Vibration fatigue of film cooling hole structure of Ni-based single crystal turbine blade: Failure behavior and life prediction [J]. Eng. Fract. Mech., 2024, 312: 110637
doi: 10.1016/j.engfracmech.2024.110637
|
| [99] |
Zhao Y J, Qu Y X, Yang W Z, et al. Vibration fatigue behavior and failure mechanism of Ni-based single-crystal film cooling hole structure under high temperature [J]. Int. J. Fatigue, 2025, 190: 108646
doi: 10.1016/j.ijfatigue.2024.108646
|
| [100] |
Li H T, Wang X M, Cheng H, et al. A systematical investigation on the impact of coupling crystal orientations on vibration characteristics of a single crystal superalloy cooling turbine blade [J]. Thin-Walled Struct., 2025, 206: 112690
doi: 10.1016/j.tws.2024.112690
|
| [101] |
Liu L, Sun S Y, Chen H T, et al. Effects of shot peening on improving high-temperature fretting fatigue performance of nickel-based single crystal superalloy tenon attachment [J]. Int. J. Fatigue, 2024, 188: 108540
doi: 10.1016/j.ijfatigue.2024.108540
|
| [102] |
Dao V H, Yun H S, Jeon S K, et al. Comparison of fatigue characteristics and failure analysis of Ni-based superalloy subjected to thermomechanical fatigue under different phase conditions [J]. Eng. Fail. Anal., 2024, 165: 108814
doi: 10.1016/j.engfailanal.2024.108814
|
| [103] |
Moverare J J, Johansson S, Reed R C. Deformation and damage mechanisms during thermal-mechanical fatigue of a single-crystal superalloy [J]. Acta Mater., 2009, 57: 2266
doi: 10.1016/j.actamat.2009.01.027
|
| [104] |
Hong H U, Kang J G, Choi B G, et al. A comparative study on thermomechanical and low cycle fatigue failures of a single crystal nickel-based superalloy [J]. Int. J. Fatigue, 2011, 33: 1592
doi: 10.1016/j.ijfatigue.2011.07.009
|
| [105] |
Segersäll M, Deng D Y. A comparative study between in- and out-of-phase thermomechanical fatigue behaviour of a single-crystal superalloy [J]. Int. J. Fatigue, 2021, 146: 106162
doi: 10.1016/j.ijfatigue.2021.106162
|
| [106] |
Wang L N, Liu Y, Yu J J, et al. Orientation and temperature dependence of yielding and deformation behavior of a nickel-base single crystal superalloy [J]. Mater. Sci. Eng., 2009, A505: 144
|
| [107] |
Vattré A, Devincre B, Roos A. Orientation dependence of plastic deformation in nickel-based single crystal superalloys: Discrete-continuous model simulations [J]. Acta Mater., 2010, 58: 1938
doi: 10.1016/j.actamat.2009.11.037
|
| [108] |
Luo C, Yuan H. Life assessment of anisotropic low cycle fatigue of nickel-base single crystal superalloy [J]. Int. J. Fatigue, 2023, 167: 107310
doi: 10.1016/j.ijfatigue.2022.107310
|
| [109] |
Gabb T P, Gayda J, Miner R V. Orientation and temperature dependence of some mechanical properties of the single-crystal nickel-base superalloy René N4 Part II. Low cycle fatigue behavior [J]. Metall. Trans., 1986, 17A: 497
|
| [110] |
Zhou H G, Luo H Y. Full-stage low cycle fatigue failure mechanisms of [001], [011] and [111] oriented single crystal superalloys by a combination of SEM, TEM and acoustic emission [J]. Mater. Sci. Eng., 2025, A922: 147596
|
| [111] |
Qu P F, Yang W C, Wang Q, et al. Unveiling the orientation sensitivity of creep life in near [001] oriented Ni-based single crystal superalloys at intermediate temperatures [J]. Int. J. Plast., 2024, 179: 104035
doi: 10.1016/j.ijplas.2024.104035
|
| [112] |
Yu J, Li J R, Zhao J Q, et al. Orientation dependence of creep properties and deformation mechanism in DD6 single crystal superalloy at 760 oC and 785 MPa [J]. Mater. Sci. Eng., 2013, A560: 47
|
| [113] |
Segersäll M, Moverare J J, Simonsson K, et al. Deformation and damage mechanisms during thermomechanical fatigue of a single-crystal superalloy in the <001> and <011> directions [A]. Superalloys 2012: 12th Internatioal Symposium on Superalloys [M]. Warrendale, PA: TMS, 2012: 215
|
| [114] |
Segersäll M, Leidermark D, Moverare J J. Influence of crystal orientation on the thermomechanical fatigue behaviour in a single-crystal superalloy [J]. Mater. Sci. Eng., 2015, A623: 68
|
| [115] |
Luo C, Yuan H. Anisotropic thermomechanical fatigue of a nickel-base single-crystal superalloy Part I: Effects of crystal orientations and damage mechanisms [J]. Int. J. Fatigue, 2023, 168: 107438
doi: 10.1016/j.ijfatigue.2022.107438
|
| [116] |
Kersey R K, Staroselsky A, Dudzinski D C, et al. Thermomechanical fatigue crack growth from laser drilled holes in single crystal nickel based superalloy [J]. Int. J. Fatigue, 2013, 55: 183
doi: 10.1016/j.ijfatigue.2013.06.006
|
| [117] |
Wang R Q, Zhang B, Hu D Y, et al. In-phase thermomechanical fatigue lifetime prediction of nickel-based single crystal superalloys from smooth specimens to notched specimens based on coupling damage on critical plane [J]. Int. J. Fatigue, 2019, 126: 327
doi: 10.1016/j.ijfatigue.2019.05.016
|
| [118] |
Zhang B, Jin X T, Zhao Y, et al. Damage simulation and experimental verification of thermomechanical fatigue in nickel-based single crystal turbine blades considering the influence of transverse crystal orientation [J]. Int. J. Fatigue, 2025, 194: 108838
doi: 10.1016/j.ijfatigue.2025.108838
|
| [119] |
Segersäll M, Kontis P, Pedrazzini S, et al. Thermal-mechanical fatigue behaviour of a new single crystal superalloy: Effects of Si and Re alloying [J]. Acta Mater., 2015, 95: 456
doi: 10.1016/j.actamat.2015.03.060
|
| [120] |
Ge Z C, Xie G, Segersäll M, et al. Influence of Ru on the thermomechanical fatigue deformation behavior of a single crystal superalloy [J]. Int. J. Fatigue, 2022, 156: 106634
doi: 10.1016/j.ijfatigue.2021.106634
|
| [121] |
Itoh Y, Saitoh M, Ishiwata Y. Influence of high-temperature protective coatings on the mechanical properties of nickel-based superalloys [J]. J. Mater. Sci., 1999, 34: 3957
doi: 10.1023/A:1004643311001
|
| [122] |
Walston W S, Schaeffer J C, Murphy W H. A new type of microstructural instability in superalloys - SRZ [A]. Superalloys 1996 [M]. Warrendale, PA: TMS, 1996: 9
|
| [123] |
Shi D Q, Song J N, Qi H Y, et al. Effect of interface diffusion on low-cycle fatigue behaviors of MCrAlY coated single crystal superalloys [J]. Int. J. Fatigue, 2020, 137: 105660
doi: 10.1016/j.ijfatigue.2020.105660
|
| [124] |
Lavigne O, Ramusat C, Drawin S, et al. Relationships between microstructural instabilities and mechanical behaviour in new generation nickel-based single crystal superalloys [A]. Superalloys 2004 [M]. Warrendale, PA: TMS, 2004: 667
|
| [125] |
Tzimas E, Müllejans H, Peteves S D, et al. Failure of thermal barrier coating systems under cyclic thermomechanical loading [J]. Acta Mater., 2000, 48: 4699
doi: 10.1016/S1359-6454(00)00260-3
|
| [126] |
Peichl A, Beck T, Vöhringer O. Behaviour of an EB-PVD thermal barrier coating system under thermal-mechanical fatigue loading [J]. Surf. Coat. Technol., 2003, 162: 113
doi: 10.1016/S0257-8972(02)00698-9
|
| [127] |
Baufeld B, Tzimas E, Hähner P, et al. Phase-angle effects on damage mechanisms of thermal barrier coatings under thermomechanical fatigue [J]. Scr. Mater., 2001, 45: 859
doi: 10.1016/S1359-6462(01)01106-X
|
| [128] |
Mauget F, Hamon F, Morisset M, et al. Damage mechanisms in an EB-PVD thermal barrier coating system during TMF and TGMF testing conditions under combustion environment [J]. Int. J. Fatigue, 2017, 99: 225
doi: 10.1016/j.ijfatigue.2016.08.001
|
| [129] |
Bartsch M, Baufeld B, Dalkiliç S, et al. Fatigue cracks in a thermal barrier coating system on a superalloy in multiaxial thermomechanical testing [J]. Int. J. Fatigue, 2008, 30: 211
doi: 10.1016/j.ijfatigue.2007.01.037
|
| [130] |
Baufeld B, Bartsch M, Dalkiliç S, et al. Defect evolution in thermal barrier coating systems under multi-axial thermomechanical loading [J]. Surf. Coat. Technol., 2005, 200: 1282
doi: 10.1016/j.surfcoat.2005.07.098
|
| [131] |
Zhan X, Wang D, Xie G, et al. Damage of thermal barrier coated superalloy under thermal gradient mechanical fatigue [A]. Superalloys 2024: Proceedings of the 15th International Symposium on Superalloys [M]. Cham: Springer, 2024: 636
|
| [132] |
Manero A, Sofronsky S, Knipe K, et al. Monitoring local strain in a thermal barrier coating system under thermal mechanical gas turbine operating conditions [J]. JOM, 2015, 67: 1528
doi: 10.1007/s11837-015-1399-3
|
| [133] |
Zhang W Q, Chen S, Guo G H, et al. Study on plastic deformation mechanism of a fourth-generation nickel-based single crystal superalloy: In-situ SEM characterization and dislocation density-based model [J]. Mater. Sci. Eng., 2025, A930: 148132
|
| [134] |
Yang X D, Zhang J B, Li W, et al. Research on the atomic-scale fracture mechanism of nickel-based superalloy DD6 at high temperature by a new in-situ technique in transmission electron microscopy [J]. J. Mater. Res. Technol., 2024, 33: 8967
doi: 10.1016/j.jmrt.2024.11.194
|
| [135] |
Tréhorel R, Ribarik G, Schenk T, et al. Real-time study of transients during high-temperature creep of an Ni-base superalloy by far-field high-energy synchrotron X-ray diffraction [J]. J. Appl. Cryst., 2018, 51: 1274
doi: 10.1107/S1600576718010014
|
| [136] |
Bruno G, Schumacher G, Pinto H C, et al. Measurement of the lattice misfit of the nickel-base superalloy SC16 by high-energy synchrotron radiation [J]. Metall. Mater. Trans., 2003, 34A: 193
|
| [137] |
Ge Z C, Xie G, Lu Y Z, et al. Influence of Ta on the intermediate temperature creep behavior of a single crystal superalloy [J]. Mater. Sci. Eng., 2022, A831: 142160
|
| [138] |
le Graverend J B, Jacques A, Cormier J, et al. Creep of a nickel-based single-crystal superalloy during very high-temperature jumps followed by synchrotron X-ray diffraction [J]. Acta Mater., 2015, 84: 65
doi: 10.1016/j.actamat.2014.10.036
|
| [139] |
Jacques A, Bastie P. The evolution of the lattice parameter mismatch of a nickel-based superalloy during a high-temperature creep test [J]. Philos. Mag., 2003, 83: 3005
doi: 10.1080/1478643031000149108
|
| [140] |
Lu Y, Ma S, Majumdar B S. Elastic microstrains during tension and creep of superalloys: Results from in situ neutron diffraction [A]. Superalloys 2008 [M]. Champion, PA: TMS, 2008: 553
|
| [141] |
Strunz P, Schumacher G, Klingelhöffer H, et al. In situ observation of morphological changes of γ′ precipitates in a pre-deformed single-crystal Ni-base superalloy [J]. J. Appl. Cryst., 2011, 44: 935
doi: 10.1107/S0021889811028147
|
| [142] |
Ratel N, Bruno G, Demé B. In situ small-angle neutron scattering investigation of the γ′ precipitation and growth in the nickel-based single-crystal alloy SC16 [J]. J. Phys.: Condens. Matter, 2005, 17: 7061
doi: 10.1088/0953-8984/17/43/022
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
| |
Shared |
|
|
|
|
| |
Discussed |
|
|
|
|