Abstract The hot deformation behavior of Ni76Cr19AlTi alloy was studied by
compression test of cylindrical specimen at constant temperature
and constant strain rate in a Gleeble-1500 system. The deformation
temperature ranges from 800 ℃ to 1150 ℃, strain rate from
10 -3 s -1 to 1 s -1. The
results show that Ni76Cr19AlTi alloy has a large deformed resistance and
is easily fractured when deformed at 800℃ and 850℃. But when compressing
at a temperature range of 950--1150℃, the resistance to deformation
reduces and the alloy doesn't fracture
because of dynamic crystallization. The measurement of the flow
stress of the alloy in high temperature range of 950-1150 ℃ showed that
the thermal deformation activation
energy Q is 376.84 kJ/mol and stress exponent n is 4.15. By analyzing the
true stress-strain curves for the alloy at hot compression and
its deformation mechanism, the suitable deformation condition is
at the temperature range from 1050 ℃ to 1150 ℃ with
strain rate from 10 -1 s -1 to 10 0 s -1.
|
|
Received: 15 August 2005
|
|
|
[1] Srinivasan N, Prasad Y V R K. J Mater Process Technol, 1995; 51: 171 [2] Choudhury I A, El-Baradie M A. J Mater Process Tech- nol, 1998; 77: 278 [3] Gabrisch H, Mukherji D. Acta Mater, 2000; 48: 3157 [4] Tian B, Paris O, Zickler G A, Lind C, Wasle G, May R P. Scr Mater, 2002; 47: 25 [5] Nembach E, Pesicka J, Langmaack E. Mater Sci Eng, 2003; A362: 264 [6] Kim D K, Kim D Y, Ryu S H, Kim D J. J Mater Process Technol, 2001; 113: 148 [7] Hagiwara Y, Ishida M, Oka T, Watanabe R, Sato K. SAE Trans, 1991; 100: 484 [8] Takagi Y, Oka.be M, Likubo T. Stahl Eisen, 1990; (Spec): 138 [9] Zener C, Hollomon J H. J Appl Phys, 1944; 15(1): 22 [10] Sellars C M. Acta Metall, 1966; 14: 1136 [11] Sellars C M, Tegart W J. Int Metall Rev, 1972; 17: 1 [12] Bruni C, Forcellese A, Gabrielli F. J Mater Process Technol, 2002; 125-126: 242 [13] Prasad Y V R K, Sasidhara S, Sikka V K. Intermetallics, 2000; 8: 987 [14] Park N K, Kim I S, Na Y S, Yeom J T. J Mater Process Technol, 2001; 111: 98 [15] Zhang B J, Zhao G P, Jiao L Y, Xu G H, Qin H Y, Feng D. Acta Metall Sin, 2005; 41: 351 (张北江,赵光普,焦兰英,胥国华,秦鹤勇,冯 涤.金属学 报,2005;41:351) |
| No Suggested Reading articles found! |
|
|
Viewed |
|
|
|
Full text
|
|
|
|
|
Abstract
|
|
|
|
|
Cited |
|
|
|
|
| |
Shared |
|
|
|
|
| |
Discussed |
|
|
|
|