| Investigation of Hot Corrosion of (Al,Mn)3Ti-2V Intermetallics |
| JIN Guangxi; LI Jinxu; QI Huibin; QIAO Lijie; GAO Kewei; HASHIMOTO Kenki; CHU Wuyang |
| Department of Materials Physics; University of Science and Technology Beijing; Beijing 100083; Japan Society for the Promotion of Science; Tokyo 102-8471; Japan |
|
Cite this article:
JIN Guangxi; LI Jinxu; QI Huibin; QIAO Lijie; GAO Kewei; HASHIMOTO Kenki; CHU Wuyang. Investigation of Hot Corrosion of (Al,Mn)3Ti-2V Intermetallics. Acta Metall Sin, 2004, 40(2): 185-190 .
|
|
|
Abstract Hot corrosion behaviors of (Al, Mn)3Ti-2V and TiAl in (Na, K)2SO4
melt at 900℃ and in Na2SO4+NaCl melt at 850℃ were studied
respectively. The cross-sectional morphologies and profiles of elements
in the scale formed on (Al, Mn)3Ti-2V show that (Al, Mn)3Ti-2V
has excellent hot
corrosion resistance in (Na, K)2SO4 melt. The thin scale
consists of an outer protective Al2O3 layer and an inner
mixture layer of Al2O3, TiO2 and TiS. When NaCl was
added in the Na2SO4 salts, however, the hot corrosion
resistance of the (Al, Mn)3Ti-2V becomes very poor. The scale is
thicker than that in the absence of NaCl by one hundred times of
magnitude at least. The scale consists of three layers: an outer
layer consisting of porous MnO plus a little Al2O3+TiO2,
a middle layer of porous Al2O3 plus trace amount of TiS,
and an inner layer of TiO2+TiS.
|
|
Received: 17 March 2003
|
|
|
[1] Raman A, Schubert K. Z Metallkd, 1965; 56: 40 [2] Chen X F, Wu X H, Chen S P, Hu G X. Scr Metall Mater, 1992: 26: 1775 [31 Hashimoto K. National Research Institute for Metals Research Activities, Japan, 2000: 30 [4] Jin G X, Kimura T, Gao K W, Hashimoto K, Qiao L J. Mater Trans JIM, 2002; 43: 2600 [5] Trethewey K R, Chamberlain J. Corrosion. Essex, England: Longman Group UK Limited. 1988: 352 [6] Yao Z, Marck M. Mater Sci Eng, 1995: A192/193: 994 [7] Nicholls J R, Legget T, Andrews P. Mater Corrs. 1997: 48: 56 [8] Tang Z L, Wang F H, Wu W T. Oxid Met, 1999; 51: 314 [9] Hara M, Hieda D, Hinata Y. J Jpn Inst Met, 1999; 63: 1238(原基,稗田大辅,日向幸昌.日本金属学会志,1999;63:1238) [10] Gocbel J A, Pettit F S, Goward G W. Metall Trans, 1973; 4: 265 [11] Jose P D, Gupta D K, Rapp A. J Electrochem Soc, 1985; 132: 735 |