| 金属材料晶界结构的拓扑性质与表征 |
朱思瑛( ), 易敏, 郭万林( ) |
| 南京航空航天大学 航空航天结构力学及控制全国重点实验室 南京 210016 |
|
| Topological Properties and Characteristics of Grain Boundary Structure in Metallic Materials |
ZHU Siying( ), YI Min, GUO Wanlin( ) |
| State Key Lab of Mechanics and Control for Aerospace Structures, Nanjing University of Aeronautics and Astronautics, Nanjing 210016, China |
引用本文:
朱思瑛, 易敏, 郭万林. 金属材料晶界结构的拓扑性质与表征[J]. 金属学报, 2026, 62(5): 705-720.
Siying ZHU,
Min YI,
Wanlin GUO.
Topological Properties and Characteristics of Grain Boundary Structure in Metallic Materials[J]. Acta Metall Sin, 2026, 62(5): 705-720.
| [1] |
Zhu S Y, Borodin E, Jivkov A P. Topological characteristics of grain boundary networks during severe plastic deformations of copper alloys [J]. Acta Mater., 2023, 259: 119290
doi: 10.1016/j.actamat.2023.119290
|
| [2] |
Devulapalli V, Chen E Z, Brink T, et al. Topological grain boundary segregation transitions [J]. Science, 2024, 386: 420
doi: 10.1126/science.adq4147
pmid: 39446949
|
| [3] |
Rohrer G S. Grain boundary energy anisotropy: A review [J]. J. Mater. Sci., 2011, 46: 5881
doi: 10.1007/s10853-011-5677-3
|
| [4] |
Gleiter H. On the structure of grain boundaries in metals [J]. Mater. Sci. Eng., 1982, 52: 91
doi: 10.1016/0025-5416(82)90040-4
|
| [5] |
Priester L. Grain Boundaries: From Theory to Engineering [M]. New York: Springer, 2012: 1
|
| [6] |
Randle V. The Measurement of Grain Boundary Geometry [M]. Boca Raton: CRC Press, 2017: 1
|
| [7] |
Han J, Thomas S L, Srolovitz D J. Grain-boundary kinetics: A unified approach [J]. Prog. Mater. Sci., 2018, 98: 386
doi: 10.1016/j.pmatsci.2018.05.004
|
| [8] |
Schuh C A, Lu K. Stability of nanocrystalline metals: The role of grain-boundary chemistry and structure [J]. MRS Bull., 2021, 46: 225
doi: 10.1557/s43577-021-00055-x
|
| [9] |
Palumbo G, Aust K T. Structure-dependence of intergranular corrosion in high purity nickel [J]. Acta Metall. Mater., 1990, 38: 2343
doi: 10.1016/0956-7151(90)90101-L
|
| [10] |
Liu G H, Wang W G, Rohrer G S, et al. {111}/{111} near singular boundaries in a dynamically recrystallized Al-Zn-Mg-Cu alloy compressed at elevated temperature [J]. Acta Metall. Sin., 2024, 60: 1165
|
| [10] |
刘光辉, 王卫国, Rohrer G S 等. 高温压缩变形Al-Zn-Mg-Cu合金动态再结晶后的{111}/{111}近奇异晶界 [J]. 金属学报, 2024, 60: 1165
doi: 10.11900/0412.1961.2023.00170
|
| [11] |
Wang G J, Vitek V. Relationships between grain boundary structure and energy [J]. Acta Metall., 1986, 34: 951
doi: 10.1016/0001-6160(86)90068-4
|
| [12] |
Bulatov V V, Reed B W, Kumar M. Grain boundary energy function for fcc metals [J]. Acta Mater., 2014, 65: 161
doi: 10.1016/j.actamat.2013.10.057
|
| [13] |
Ratanaphan S, Olmsted D L, Bulatov V V, et al. Grain boundary energies in body-centered cubic metals [J]. Acta Mater., 2015, 88: 346
doi: 10.1016/j.actamat.2015.01.069
|
| [14] |
Chen K T, Srolovitz D J, Han J. Grain-boundary topological phase transitions [J]. Proc. Natl. Acad. Sci. USA, 2020, 117: 33077
doi: 10.1073/pnas.2017390117
pmid: 33318180
|
| [15] |
Wang J W, Chen Y B, Zhu Q, et al. Grain boundary dominated plasticity in metallic materials [J]. Acta Metall. Sin., 2022, 58: 726
doi: 10.11900/0412.1961.2021.00594
|
| [15] |
王江伟, 陈映彬, 祝 祺 等. 金属材料的晶界塑性变形机制 [J]. 金属学报, 2022, 58: 726
doi: 10.11900/0412.1961.2021.00594
|
| [16] |
Reed B W, Kumar M, Minich R W, et al. Fracture roughness scaling and its correlation with grain boundary network structure [J]. Acta Mater., 2008, 56: 3278
doi: 10.1016/j.actamat.2008.03.019
|
| [17] |
Gao Y, Liu X, Wang Y Q, et al. The role of special grain boundaries in enhancing creep performance in the welded joint of a novel Fe-Ni-based superalloy through aging treatment [J]. Mater. Charact., 2025, 224: 115010
doi: 10.1016/j.matchar.2025.115010
|
| [18] |
Zheng X Y, Chen X, He M L, et al. Multi-scale simulation of mechanical properties of 6XXX aluminum alloy based on crystal plasticity [J]. Acta Metall. Sin., 2025, 61: 1758
doi: 10.11900/0412.1961.2024.00083
|
| [18] |
郑潇禹, 陈 辛, 何美玲 等. 基于晶体塑性的6XXX铝合金力学性能多尺度计算 [J]. 金属学报, 2025, 61: 1758
doi: 10.11900/0412.1961.2024.00083
|
| [19] |
Hu C Z, Li Y W, Yu Z Y, et al. Computing grain boundary diagrams of thermodynamic and mechanical properties [J]. npj Comput. Mater., 2021, 7: 159
doi: 10.1038/s41524-021-00625-2
|
| [20] |
Marquardt K, Rohrer G S, Morales L, et al. The most frequent interfaces in olivine aggregates: The GBCD and its importance for grain boundary related processes [J]. Contrib. Mineral. Petrol., 2015, 170: 40
doi: 10.1007/s00410-015-1193-9
|
| [21] |
Chookajorn T, Murdoch H A, Schuh C A. Design of stable nanocrystalline alloys [J]. Science, 2012, 337: 951
doi: 10.1126/science.1224737
pmid: 22923577
|
| [22] |
Garner A, Euesden R, Yao Y C, et al. Multiscale analysis of grain boundary microstructure in high strength 7xxx Al alloys [J]. Acta Mater., 2021, 202: 190
doi: 10.1016/j.actamat.2020.10.021
|
| [23] |
Wilde G, Divinski S. Grain boundaries and diffusion phenomena in severely deformed materials [J]. Mater. Trans., 2019, 60: 1302
doi: 10.2320/matertrans.MF201934
|
| [24] |
Leitner K, Lutz D, Knabl W, et al. Grain boundary segregation engineering in as-sintered molybdenum for improved ductility [J]. Scr. Mater., 2018, 156: 60
doi: 10.1016/j.scriptamat.2018.07.008
|
| [25] |
Zhu Y L, Cao Y, Tian W, et al. New insights into ductility improvement of a nickel-based superalloy through grain boundary engineering [J]. Mater. Sci. Eng., 2024, A908: 146786
|
| [26] |
Tikhonova M, Kaibyshev R, Belyakov A. Microstructure and mechanical properties of austenitic stainless steels after dynamic and post-dynamic recrystallization treatment [J]. Adv. Eng. Mater., 2018, 20: 1700960
doi: 10.1002/adem.v20.7
|
| [27] |
Zhuo Z, Xia S, Bai Q, et al. The effect of grain boundary character distribution on the mechanical properties at different strain rates of a 316L stainless steel [J]. J. Mater. Sci., 2018, 53: 2844
doi: 10.1007/s10853-017-1695-0
|
| [28] |
Naydenkin E V, Ratochka I V, Mishin I P, et al. The effect of interfaces on mechanical and superplastic properties of titanium alloys [J]. J. Mater. Sci., 2017, 52: 4164
doi: 10.1007/s10853-016-0508-1
|
| [29] |
Li L L, Zhang P, Zhang Z J, et al. Strain localization and fatigue cracking behaviors of Cu bicrystal with an inclined twin boundary [J]. Acta Mater., 2014, 73: 167
doi: 10.1016/j.actamat.2014.04.004
|
| [30] |
Jin Y J, Lu H, Yu C, et al. Study on grain boundary character and strain distribution of intergranular cracking in the CGHAZ of T23 steel [J]. Mater. Charact., 2013, 84: 216
doi: 10.1016/j.matchar.2013.08.004
|
| [31] |
Das A. Grain boundary engineering: fatigue fracture [J]. Philos. Mag., 2017, 97: 867
doi: 10.1080/14786435.2017.1285072
|
| [32] |
Lu K. Stabilizing nanostructures in metals using grain and twin boundary architectures [J]. Nat. Rev. Mater., 2016, 1: 16019
doi: 10.1038/natrevmats.2016.19
|
| [33] |
Van Swygenhoven H. Grain boundaries and dislocations [J]. Science, 2002, 296: 66
pmid: 11935012
|
| [34] |
Hirth J P. The influence of grain boundaries on mechanical properties [J]. Metall. Trans., 1972, 3: 3047
|
| [35] |
Palumbo G, Lehockey E M, Lin P. Applications for grain boundary engineered materials [J]. JOM, 1998, 50(2): 40
|
| [36] |
Randle V, Ralph B. Grain boundary structure and mechanical properties [J]. Rev. Phys. Appl., 1988, 23: 501
|
| [37] |
Kheradmand N, Barnoush A, Vehoff H. Investigation of the role of grain boundary on the mechanical properties of metals [J]. J. Phys.: Conf. Ser., 2010, 240: 012017
|
| [38] |
Randle V, Owen G. Mechanisms of grain boundary engineering [J]. Acta Mater., 2006, 54: 1777
doi: 10.1016/j.actamat.2005.11.046
|
| [39] |
Randle V. ‘Special’ boundaries and grain boundary plane engineering [J]. Scr. Mater., 2006, 54: 1011
doi: 10.1016/j.scriptamat.2005.11.050
|
| [40] |
Randle V. Grain boundary engineering: An overview after 25 years [J]. Mater. Sci. Technol., 2010, 26: 253
doi: 10.1179/026708309X12601952777747
|
| [41] |
Watanabe T. Grain boundary engineering: Historical perspective and future prospects [J]. J. Mater. Sci., 2011, 46: 4095
doi: 10.1007/s10853-011-5393-z
|
| [42] |
Raabe D, Herbig M, Sandlöbes S, et al. Grain boundary segregation engineering in metallic alloys: A pathway to the design of interfaces [J]. Curr. Opin. Solid State Mater. Sci., 2014, 18: 253
doi: 10.1016/j.cossms.2014.06.002
|
| [43] |
Xu X M, Zhong Y J, Wajrak M, et al. Grain boundary engineering: An emerging pathway toward efficient electrocatalysis [J]. InfoMat, 2024, 6: e12608
doi: 10.1002/inf2.12608
|
| [44] |
Tiamiyu A A, Pang E L, Chen X, et al. Nanotwinning-assisted dynamic recrystallization at high strains and strain rates [J]. Nat. Mater., 2022, 21: 786
doi: 10.1038/s41563-022-01250-0
pmid: 35590039
|
| [45] |
Figueiredo R B, Langdon T G. Fabricating ultrafine-grained materials through the application of severe plastic deformation: A review of developments in brazil [J]. J. Mater. Res. Technol., 2012, 1: 55
doi: 10.1016/S2238-7854(12)70010-8
|
| [46] |
Panzarino J F, Pan Z L, Rupert T J. Plasticity-induced restructuring of a nanocrystalline grain boundary network [J]. Acta Mater., 2016, 120: 1
doi: 10.1016/j.actamat.2016.08.040
|
| [47] |
Fu H L, Zhou X, Gao Z P, et al. Effect of grain geometry on the stability of polycrystalline Pt at the nanoscale [J]. Phys. Rev. Lett., 2025, 134: 056101
|
| [48] |
Zhang L, Lu C, Tieu K. A review on atomistic simulation of grain boundary behaviors in face-centered cubic metals [J]. Comput. Mater. Sci., 2016, 118: 180
doi: 10.1016/j.commatsci.2016.03.021
|
| [49] |
Pan X L, Zhou L C, Wang C X, et al. Microstructure and residual stress modulation of 7075 aluminum alloy for improving fatigue performance by laser shock peening [J]. Int. J. Mach. Tools Manuf., 2023, 184: 103979
doi: 10.1016/j.ijmachtools.2022.103979
|
| [50] |
Abdeljawad F, Foiles S M, Moore A P, et al. The role of the interface stiffness tensor on grain boundary dynamics [J]. Acta Mater., 2018, 158: 440
doi: 10.1016/j.actamat.2018.06.025
|
| [51] |
Randle V. The Role of the Coincidence Site Lattice in Grain Boundary Engineering [M]. London: CRC Press, 2024: 1
|
| [52] |
Lee D S, Ryoo H S, Hwang S K. A grain boundary engineering approach to promote special boundaries in Pb-base alloy [J]. Mater. Sci. Eng., 2003, A354: 106
|
| [53] |
Warren P, Raju N, Prasad A, et al. Grain and grain boundary segmentation using machine learning with real and generated datasets [J]. Comput. Mater. Sci., 2024, 233: 112739
doi: 10.1016/j.commatsci.2023.112739
|
| [54] |
Zhu Q, Samanta A, Li B X, et al. Predicting phase behavior of grain boundaries with evolutionary search and machine learning [J]. Nat. Commun., 2018, 9: 467
doi: 10.1038/s41467-018-02937-2
pmid: 29391453
|
| [55] |
Huber L, Hadian R, Grabowski B, et al. A machine learning approach to model solute grain boundary segregation [J]. npj Comput. Mater., 2018, 4: 64
doi: 10.1038/s41524-018-0122-7
|
| [56] |
Zhang J N, Koneru A, Sankaranarayanan S K R S, et al. Graph neural network guided evolutionary search of grain boundaries in 2D materials [J]. ACS Appl. Mater. Interfaces, 2023, 15: 20520
doi: 10.1021/acsami.3c01161
|
| [57] |
van Beers P R M, Kouznetsova V G, Geers M G D, et al. A multiscale model of grain boundary structure and energy: From atomistics to a continuum description [J]. Acta Mater., 2015, 82: 513
doi: 10.1016/j.actamat.2014.08.045
|
| [58] |
Song X Y, Deng C. Atomic energy in grain boundaries studied by machine learning [J]. Phys. Rev. Mater., 2022, 6: 043601
|
| [59] |
Patala S. Topological analysis of the grain boundary space [D]. Cambridge: Massachusetts Institute of Technology, 2011
|
| [60] |
Wakai F, Shinoda Y, Ishihara S, et al. Topological transformation of grains in three-dimensional normal grain growth [J]. J. Mater. Res., 2001, 16: 2136
doi: 10.1557/JMR.2001.0291
|
| [61] |
Gao N N, Zhao Y, Xia W Q, et al. Phase-field crystal studies on grain boundary migration, dislocation behaviors, and topological transition under tension of square polycrystals [J]. Crystals, 2023, 13: 777
doi: 10.3390/cryst13050777
|
| [62] |
Narang P, Garcia C A C, Felser C. The topology of electronic band structures [J]. Nat. Mater., 2021, 20: 293
doi: 10.1038/s41563-020-00820-4
pmid: 33139890
|
| [63] |
Gupta S, Saxena A. A topological twist on materials science [J]. MRS Bull., 2014, 39: 265
doi: 10.1557/mrs.2014.28
|
| [64] |
Hirth J P, Balluffi R W. On grain boundary dislocations and ledges [J]. Acta Metall., 1973, 21: 929
doi: 10.1016/0001-6160(73)90150-8
|
| [65] |
Gleiter H. Nanostructured materials: Basic concepts and microstructure [J]. Acta Mater., 2000, 48: 1
doi: 10.1016/S1359-6454(99)00285-2
|
| [66] |
Zhu Q, Zhao Q K, Huang Q S, et al. Grain boundary plasticity initiated by excess volume [J]. Proc. Natl. Acad. Sci. USA, 2024, 121: e2400161121
doi: 10.1073/pnas.2400161121
|
| [67] |
Ma K K, Wen H M, Hu T, et al. Mechanical behavior and strengthening mechanisms in ultrafine grain precipitation-strengthened aluminum alloy [J]. Acta Mater., 2014, 62: 141
doi: 10.1016/j.actamat.2013.09.042
|
| [68] |
Hellman O C, Vandenbroucke J A, Rüsing J, et al. Analysis of three-dimensional atom-probe data by the proximity histogram [J]. Microsc. Microanal., 2000, 6: 437
pmid: 11003678
|
| [69] |
Wagih M, Larsen P M, Schuh C A. Learning grain boundary segregation energy spectra in polycrystals [J]. Nat. Commun., 2020, 11: 6376
doi: 10.1038/s41467-020-20083-6
pmid: 33311515
|
| [70] |
Wei C Z, Thomas S L, Han J, et al. A continuum multi-disconnection-mode model for grain boundary migration [J]. J. Mech. Phys. Solids, 2019, 133: 103731
doi: 10.1016/j.jmps.2019.103731
|
| [71] |
Wang L H, Zhang Y, Zeng Z, et al. Tracking the sliding of grain boundaries at the atomic scale [J]. Science, 2022, 375: 1261
doi: 10.1126/science.abm2612
pmid: 35298254
|
| [72] |
Lu K. Gradient nanostructured materials [J]. Acta Metall. Sin., 2015, 51: 1
doi: 10.11900/0412.1961.2014.00395
|
| [72] |
卢 柯. 梯度纳米结构材料 [J]. 金属学报, 2015, 51: 1
|
| [73] |
Fu H L, Zhou X, Gao Z P, et al. Pt Schwarz crystals stabilized by minimal-surface grain boundaries and twins at the grain size limit [J]. Acta Mater., 2024, 276: 120007
doi: 10.1016/j.actamat.2024.120007
|
| [74] |
Lu L, Shen Y F, Chen X H, et al. Ultrahigh strength and high electrical conductivity in copper [J]. Science, 2004, 304: 422
pmid: 15031435
|
| [75] |
Zhu Q, Huang Q S, Guang C, et al. Metallic nanocrystals with low angle grain boundary for controllable plastic reversibility [J]. Nat. Commun., 2020, 11: 3100
doi: 10.1038/s41467-020-16869-3
pmid: 32555195
|
| [76] |
Cantwell P R, Tang M, Dillon S J, et al. Grain boundary complexions [J]. Acta Mater., 2014, 62: 1
doi: 10.1016/j.actamat.2013.07.037
|
| [77] |
Cantwell P R, Frolov T, Rupert T J, et al. Grain boundary complexion transitions [J]. Annu. Rev. Mater. Res., 2020, 50: 465
doi: 10.1146/annurev-matsci-081619-114055
|
| [78] |
Zhang Z B, Yang Z B, Lu S, et al. Strain localisation and failure at twin-boundary complexions in nickel-based superalloys [J]. Nat. Commun., 2020, 11: 4890
doi: 10.1038/s41467-020-18641-z
pmid: 32994396
|
| [79] |
Krause A R, Cantwell P R, Marvel C J, et al. Review of grain boundary complexion engineering: Know your boundaries [J]. J. Am. Ceram. Soc., 2019, 102: 778
doi: 10.1111/jace.16045
|
| [80] |
Grimmer H, Bollmann W, Warrington D H. Coincidence-site lattices and complete pattern-shift in cubic crystals [J]. Acta Cryst., 1974, 30A: 197
|
| [81] |
Bollmann W. Crystal Defects and Crystalline Interfaces [M]. Berlin: Springer, 2012: 1
|
| [82] |
Pond R C, Bollmann W. The symmetry and interfacial structure of bicrystals [J]. Philos. Trans. Roy. Soc., 1979, 292A: 449
|
| [83] |
Warrington D H, Bollmann W. Dislocation networks in high-angle grain boundaries [J]. Philos. Mag., 1972, 25: 1195
doi: 10.1080/14786437208226861
|
| [84] |
Bollmann W. On the geometry of grain and phase boundaries: I. General theory [J]. Philos. Mag., 1967, 16: 363
|
| [85] |
Randle V, Rohrer G S, Miller H M, et al. Five-parameter grain boundary distribution of commercially grain boundary engineered nickel and copper [J]. Acta Mater., 2008, 56: 2363
doi: 10.1016/j.actamat.2008.01.039
|
| [86] |
Ratanaphan S, Yoon Y, Rohrer G S. The five parameter grain boundary character distribution of polycrystalline silicon [J]. J. Mater. Sci., 2014, 49: 4938
doi: 10.1007/s10853-014-8195-2
|
| [87] |
An D, Griffiths T A, Konijnenberg P, et al. Correlating the five parameter grain boundary character distribution and the intergranular corrosion behaviour of a stainless steel using 3D orientation microscopy based on mechanical polishing serial sectioning [J]. Acta Mater., 2018, 156: 297
doi: 10.1016/j.actamat.2018.06.044
|
| [88] |
Brandon D G. The structure of high-angle grain boundaries [J]. Acta Metall., 1966, 14: 1479
doi: 10.1016/0001-6160(66)90168-4
|
| [89] |
Bollmann W. The basic concepts of the 0-lattice theory [J]. Surf. Sci., 1972, 31: 1
doi: 10.1016/0039-6028(72)90250-6
|
| [90] |
Bollmann W. O‐lattice calculation of an F.C.C.-B.C.C. interface [J]. Phys. Status Solidi, 1974, 21A: 543
|
| [91] |
Li M, Xu T. Topological and atomic scale characterization of grain boundary networks in polycrystalline and nanocrystalline materials [J]. Prog. Mater. Sci., 2011, 56: 864
doi: 10.1016/j.pmatsci.2011.01.011
|
| [92] |
Jin Z H, Li X Y, Lu K. Formation of stable schwarz crystals in polycrystalline copper at the grain size limit [J]. Phys. Rev. Lett., 2021, 127: 136101
doi: 10.1103/PhysRevLett.127.136101
|
| [93] |
Xu W, Zhang B, Li X Y, et al. Suppressing atomic diffusion with the Schwarz crystal structure in supersaturated Al-Mg alloys [J]. Science, 2021, 373: 683
doi: 10.1126/science.abh0700
pmid: 34353952
|
| [94] |
Gu J L, Duan F H, Liu S D, et al. Phase engineering of nanostructural metallic materials: Classification, structures, and applications [J]. Chem. Rev., 2024, 124: 1247
doi: 10.1021/acs.chemrev.3c00514
|
| [95] |
Meiners T, Frolov T, Rudd R E, et al. Observations of grain-boundary phase transformations in an elemental metal [J]. Nature, 2020, 579: 375
doi: 10.1038/s41586-020-2082-6
|
| [96] |
Zhu S Y, Jivkov A P, Borodin E, et al. Triple junction disclinations in severely deformed Cu-0.4%Mg alloys [J]. Acta Mater., 2024, 264: 119600
doi: 10.1016/j.actamat.2023.119600
|
| [97] |
Bollmann W. Triple lines in polycrystalline aggregates as disclinations [J]. Philos. Mag., 1984, 49A: 73
|
| [98] |
Bollmann W. Triple-line disclinations representations, continuity and reactions [J]. Philos. Mag., 1988, 57A: 637
|
| [99] |
Liu Y, Leung S, Li F F, et al. Bulk-disclination correspondence in topological crystalline insulators [J]. Nature, 2021, 589: 381
doi: 10.1038/s41586-020-03125-3
|
| [100] |
Wu M S, Zhou K, Nazarov A A. Crack nucleation at disclinated triple junctions [J]. Phys. Rev., 2007, 76B: 134105
|
| [101] |
Barnett A K, Hussein O, Alghalayini M, et al. Triple junction segregation dominates the stability of nanocrystalline alloys [J]. Nano Lett., 2024, 24: 9627
doi: 10.1021/acs.nanolett.4c02395
|
| [102] |
Wei C Z, Zhang C L, Han J, et al. Grain boundary triple junction dynamics: A continuum disconnection model [J]. SIAM J. Appl. Math., 2020, 80: 1101
doi: 10.1137/19M1277722
|
| [103] |
Annevelink E, Ertekin E, Johnson H T. Grain boundary structure and migration in graphene via the displacement shift complete lattice [J]. Acta Mater., 2019, 166: 67
doi: 10.1016/j.actamat.2018.12.030
|
| [104] |
Song X Q, Tang L Y, Wang Y X, et al. Plastic strain-induced evolution of CSL boundaries at elevated temperature for Ni-base superalloy: Experimental and phase-field perspective [J]. J. Mater. Res. Technol., 2020, 9: 2535
doi: 10.1016/j.jmrt.2019.12.084
|
| [105] |
Zhou S Y, Hu M H, Li C, et al. Creep behavior of a Ni-based superalloy with strengthening of γ' and γ'' phases [J]. Acta Metall. Sin., 2025, 61: 226
|
| [105] |
周生玉, 胡明昊, 李 冲 等. 一种γ'/γ''相强化镍基高温合金的蠕变行为 [J]. 金属学报, 2025, 61: 226
doi: 10.11900/0412.1961.2022.00571
|
| [106] |
Zhang Y, He C Y, Yu Q, et al. Nacre-like surface nanolaminates enhance fatigue resistance of pure titanium [J]. Nat. Commun., 2024, 15: 6917
doi: 10.1038/s41467-024-51423-5
pmid: 39134556
|
| [107] |
Zhou X Y, Ahmadian A, Gault B, et al. Atomic motifs govern the decoration of grain boundaries by interstitial solutes [J]. Nat. Commun., 2023, 14: 3535
doi: 10.1038/s41467-023-39302-x
pmid: 37316498
|
| [108] |
Schuh C A, Kumar M, King W E. Analysis of grain boundary networks and their evolution during grain boundary engineering [J]. Acta Mater., 2003, 51: 687
doi: 10.1016/S1359-6454(02)00447-0
|
| [109] |
Kumar M, King W E, Schwartz A J. Modifications to the microstructural topology in f.c.c. materials through thermomechanical processing [J]. Acta Mater., 2000, 48: 2081
doi: 10.1016/S1359-6454(00)00045-8
|
| [110] |
Farabi E, Tari V, Hodgson P D, et al. On the grain boundary network characteristics in a martensitic Ti-6Al-4V alloy [J]. J. Mater. Sci., 2020, 55: 15299
doi: 10.1007/s10853-020-05075-7
|
| [111] |
Chen Y B, Han J, Deng H L, et al. Revealing grain boundary kinetics in three-dimensional space [J]. Acta Mater., 2024, 268: 119717
doi: 10.1016/j.actamat.2024.119717
|
| [112] |
Priedeman J L, Rosenbrock C W, Johnson O K, et al. Quantifying and connecting atomic and crystallographic grain boundary structure using local environment representation and dimensionality reduction techniques [J]. Acta Mater., 2018, 161: 431
doi: 10.1016/j.actamat.2018.09.011
|
| [113] |
Palumbo G, Thorpe S J, Aust K T. On the contribution of triple junctions to the structure and properties of nanocrystalline materials [J]. Scr. Metall. Mater., 1990, 24: 1347
doi: 10.1016/0956-716X(90)90354-J
|
| [114] |
Chen E Z, Heo T W, Wood B C, et al. Grand canonically optimized grain boundary phases in hexagonal close-packed titanium [J]. Nat. Commun., 2024, 15: 7049
doi: 10.1038/s41467-024-51330-9
pmid: 39147757
|
| [115] |
Yazyev O V, Louie S G. Topological defects in graphene: Dislocations and grain boundaries [J]. Phys. Rev., 2010, 81B: 195420
|
| [116] |
Korbuly B, Plapp M, Henry H, et al. Topological defects in two-dimensional orientation-field models for grain growth [J]. Phys. Rev., 2017, 96E: 052802
|
| [117] |
Barr C M, Leff A C, Demott R W, et al. Unraveling the origin of twin related domains and grain boundary evolution during grain boundary engineering [J]. Acta Mater., 2018, 144: 281
doi: 10.1016/j.actamat.2017.10.007
|
| [118] |
Kinderlehrer D, Liu C. Evolution of grain boundaries [J]. Math. Models Methods Appl. Sci., 2001, 11: 713
doi: 10.1142/S0218202501001069
|
| [119] |
Niño J D, Johnson O K. Influence of grain boundary energy anisotropy on the evolution of grain boundary network structure during 3D anisotropic grain growth [J]. Comput. Mater. Sci, 2023, 217: 111879
doi: 10.1016/j.commatsci.2022.111879
|
| [120] |
Luo M, Liao X Z, Ringer S P, et al. Grain boundary network evolution in electron-beam powder bed fusion nickel-based superalloy Inconel 738 [J]. J. Alloys Compd., 2024, 972: 172811
doi: 10.1016/j.jallcom.2023.172811
|
| [121] |
Yang X Y, Wang P, Huang M. Grain boundary evolution during low-strain grain boundary engineering achieved by strain-induced boundary migration in pure copper [J]. Mater. Sci. Eng., 2022, A833: 142532
|
| [122] |
Volovitch P, Traskine V, Barrallier L. Analysis of grain boundary network topology using grain boundary wetting [J]. Z. Metallkd., 2004, 95: 215
doi: 10.3139/146.017935
|
| [123] |
Minich R W, Schuh C A, Kumar M. Role of topological constraints on the statistical properties of grain boundary networks [J]. Phys. Rev., 2002, 66B: 052101
|
| [124] |
Rohrer G S, Miller H M. Topological characteristics of plane sections of polycrystals [J]. Acta Mater., 2010, 58: 3805
doi: 10.1016/j.actamat.2010.03.028
|
| [125] |
Liu T G, Xia S, Zhou B X, et al. Three-dimensional geometrical and topological characteristics of grains in conventional and grain boundary engineered 316L stainless steel [J]. Micron, 2018, 109: 58
doi: S0968-4328(18)30058-1
pmid: 29665457
|
| [126] |
Li X Y, Jin Z H, Zhou X, et al. Constrained minimal-interface structures in polycrystalline copper with extremely fine grains [J]. Science, 2020, 370: 831
doi: 10.1126/science.abe1267
pmid: 33184210
|
| [127] |
Rollett A D, Lee S B, Campman R, et al. Three-dimensional characterization of microstructure by electron back-scatter diffraction [J]. Annu. Rev. Mater. Res., 2007, 37: 627
doi: 10.1146/matsci.2007.37.issue-1
|
| [128] |
Christopher W A, Oliver K J. A decision transformer approach to grain boundary network optimization [J]. Comput. Mater. Sci., 2025, 253: 113852
doi: 10.1016/j.commatsci.2025.113852
|
| [129] |
Irukuvarghula S, Hassanin H, Cayron C, et al. Evolution of grain boundary network topology in 316L austenitic stainless steel during powder hot isostatic pressing [J]. Acta Mater., 2017, 133: 269
doi: 10.1016/j.actamat.2017.04.068
|
| [130] |
Patala S, Mason J K, Schuh C A. Improved representations of misorientation information for grain boundary science and engineering [J]. Prog. Mater. Sci., 2012, 57: 1383
doi: 10.1016/j.pmatsci.2012.04.002
|
| [131] |
Johnson O K, Lund J M, Critchfield T R. Spectral graph theory for characterization and homogenization of grain boundary networks [J]. Acta Mater., 2018, 146: 42
doi: 10.1016/j.actamat.2017.11.054
|
| [132] |
Valiev R Z, Langdon T G. Principles of equal-channel angular pressing as a processing tool for grain refinement [J]. Prog. Mater. Sci., 2006, 51: 881
doi: 10.1016/j.pmatsci.2006.02.003
|
| [133] |
Winning M, Gottstein G, Shvindlerman L S. On the mechanisms of grain boundary migration [J]. Acta Mater., 2002, 50: 353
doi: 10.1016/S1359-6454(01)00343-3
|
| [134] |
Voyiadjis G Z. Grain boundary migration in metals: Thermodynamics, kinetics, applications [J]. J. Eng. Mech., 2000, 126: 888
|
| [135] |
Jia H R, Duan S Y, Zhang Z, et al. Homogenization-based topology optimization for self-supporting additive-manufactured lattice-infilled structure [J]. Mater. Des., 2024, 245: 113264
doi: 10.1016/j.matdes.2024.113264
|
| [136] |
Rohrer G S. Measuring and interpreting the structure of grain-boundary networks [J]. J. Am. Ceram. Soc., 2011, 94: 633
doi: 10.1111/jace.2011.94.issue-3
|
| [137] |
Barr C M, Thomas S, Hart J L, et al. Tracking the evolution of intergranular corrosion through twin-related domains in grain boundary networks [J]. npj Mater. Degrad., 2018, 2: 14
doi: 10.1038/s41529-018-0032-7
|
| [138] |
Liu T G, Xia S, Li H, et al. The highly twinned grain boundary network formation during grain boundary engineering [J]. Mater. Lett., 2014, 133: 97
doi: 10.1016/j.matlet.2014.06.166
|
| [139] |
Zhu X J, Fan Q B, Liu X, et al. Microstructure evolution and mechanical properties of a hot-rolled Ti alloy [J]. Prog. Nat. Sci.: Mater. Int., 2021, 31: 105
doi: 10.1016/j.pnsc.2020.11.007
|
| [140] |
Johnson O K, Schuh C A. The triple junction hull: Tools for grain boundary network design [J]. J. Mech. Phys. Solids, 2014, 69: 2
doi: 10.1016/j.jmps.2014.04.005
|
| [141] |
Frary M, Schuh C A. Connectivity and percolation behaviour of grain boundary networks in three dimensions [J]. Philos. Mag., 2005, 85: 1123
doi: 10.1080/14786430412331323564
|
| [142] |
Liang C G, Yin Y, Wang W X, et al. A thermodynamically consistent non-isothermal phase-field model for selective laser sintering [J]. Int. J. Mech. Sci., 2023, 259: 108602
doi: 10.1016/j.ijmecsci.2023.108602
|
| [143] |
Zhang B B, Tang Y G, Mei Q S, et al. Inhibiting creep in nanograined alloys with stable grain boundary networks [J]. Science, 2022, 378: 659
doi: 10.1126/science.abq7739
pmid: 36356141
|
| [144] |
Bhattacharya A, Shen Y F, Hefferan C M, et al. Grain boundary velocity and curvature are not correlated in Ni polycrystals [J]. Science, 2021, 374: 189
doi: 10.1126/science.abj3210
pmid: 34618565
|
| [145] |
Lin B, Jin Y, Hefferan C M, et al. Observation of annealing twin nucleation at triple lines in nickel during grain growth [J]. Acta Mater., 2015, 99: 63
doi: 10.1016/j.actamat.2015.07.041
|
| [146] |
Liu T G, Xia S, Zhou B X, et al. Three-dimensional characteristics of the grain boundary networks of conventional and grain boundary engineered 316L stainless steel [J]. Mater. Charact., 2017, 133: 60
doi: 10.1016/j.matchar.2017.09.026
|
| [147] |
Wanner T, Fuller E R, Saylor D M. Homology metrics for microstructure response fields in polycrystals [J]. Acta Mater., 2010, 58: 102
doi: 10.1016/j.actamat.2009.08.061
|
| [148] |
Kobayashi S, Tsurekawa S, Watanabe T. A new approach to grain boundary engineering for nanocrystalline materials [J]. Beilstein J. Nanotechnol., 2016, 7: 1829
doi: 10.3762/bjnano.7.176
|
| [149] |
Yang D, Bai Q, Hu Y, et al. Fractal analysis of the effect of grain boundary character on Te-induced brittle cracking in GH3535 alloy [J]. Acta Metall. Sin., 2023, 59: 248
doi: 10.11900/0412.1961.2021.00584
|
| [149] |
杨 杜, 白 琴, 胡 悦 等. GH3535合金中晶界特征对碲致脆性开裂影响的分形分析 [J]. 金属学报, 2023, 59: 248
|
| [150] |
Zhu S Y. In silico grain boundary engineering by analysis on discrete complexes [D]. Manchester: The University of Manchester, 2023
|
| [151] |
Hatcher A. Algebraic Topology [M]. Beijing: Tsinghua University, 2005: 1
|
| [152] |
Salnikov V, Cassese D, Lambiotte R. Simplicial complexes and complex systems [J]. Eur. J. Phys., 2018, 40: 014001
|
| [153] |
Zhu S Y, Gao W J, Yi M, et al. Integrated discrete cell complexes and finite element analysis for microstructure topology evolution during severe plastic deformation [J]. Comput. Mater. Contin., 2025, 85: 657
|
|