金属学报  2025, Vol. 61 Issue (11): 1673-1688    DOI: 10.11900/0412.1961.2024.00035
  研究论文 本期目录 | 过刊浏览 |
室温和深冷轧制对纯Al再结晶{111}/{111}近奇异晶界的影响
李振想1, 王卫国1,2(), Rohrer Gregory S3, 洪丽华1,2, 陈松1,2, 林燕1,2, 周邦新4
1 福建理工大学 晶界工程研究所 福州 350118
2 福建理工大学 材料科学与工程学院 福州 350118
3 Department of Materials Science and Engineering, Carnegie Mellon University, Pittsburgh, PA15213 -3890, USA
4 上海大学 材料研究所 上海 200072
Effects of Ambient and Cryogenic Rolling on {111}/{111} Near Singular Boundary Formation During Subsequent Recrystallization Annealing in Pure Aluminum
LI Zhenxiang1, WANG Weiguo1,2(), Rohrer Gregory S3, HONG Lihua1,2, CHEN Song1,2, LIN Yan1,2, ZHOU Bangxin4
1 Institute of Grain Boundary Engineering, Fujian University of Technology, Fuzhou 350118, China
2 School of Materials Science and Technology, Fujian University of Technology, Fuzhou 350118, China
3 Department of Materials Science and Engineering, Carnegie Mellon University, Pittsburgh, PA15213 -3890, USA
4 Institute of Materials, Shanghai University, Shanghai 200072, China
引用本文:

李振想, 王卫国, Rohrer Gregory S, 洪丽华, 陈松, 林燕, 周邦新. 室温和深冷轧制对纯Al再结晶{111}/{111}近奇异晶界的影响[J]. 金属学报, 2025, 61(11): 1673-1688.
Zhenxiang LI, Weiguo WANG, Gregory S Rohrer, Lihua HONG, Song CHEN, Yan LIN, Bangxin ZHOU. Effects of Ambient and Cryogenic Rolling on {111}/{111} Near Singular Boundary Formation During Subsequent Recrystallization Annealing in Pure Aluminum[J]. Acta Metall Sin, 2025, 61(11): 1673-1688.

全文: PDF(5141 KB)   HTML
摘要: 

{111}/{111}近奇异晶界比一般晶界更耐蚀,研究此类晶界的形成条件、影响因素和生成机制,设法调控此类晶界并提高其比例是改善相关铝合金晶界间耐腐蚀性能的根本途径。为了解铝合金生成{111}/{111}近奇异晶界的本征行为,本工作选择高纯Al (99.99%)为实验材料,首先经室温反复多向锻造和370 ℃再结晶退火获得晶粒尺寸均匀(平均晶粒尺寸约为20 μm)且晶粒取向随机分布的组织均匀化初始样品;再将初始样品分别在室温(25 ℃)和-196 ℃深冷条件下进行厚度减缩量为80%的轧制变形,及370 ℃、30 min再结晶退火处理。采用EBSD和基于五参数分析的晶界界面匹配定量表征方法对2种样品进行测试和分析。结果表明,经-196 ℃深冷轧制并再结晶的样品,其{111}/{111}近奇异晶界比例达到6.0%,相比室温轧制并再结晶的样品提升了122%。XRD、EBSD及硬度测试结果表明,经室温和-196 ℃深冷轧制的样品中均形成了较强的{011}<111¯>形变织构;相比于室温轧制,经-196 ℃深冷轧制的样品内残余压应力更大,晶粒碎化更严重、储能更高。在后续370 ℃退火过程中,经室温和-196 ℃深冷轧制的样品,其再结晶机制均以{011}<011¯>取向生长为主;相比于室温轧制,经-196 ℃深冷轧制的样品可提供更大的晶界迁移驱动力,其样品再结晶组织的平均晶粒尺寸更大且{011}<011¯>再结晶织构更强。统计结果表明,{011}<011¯>取向晶粒与其他取向的晶粒毗连所形成的晶界中存在较高比例的{111}/{111}近奇异晶界;同时,{011}<011¯>取向晶粒与其相邻的且具有{011}<011¯>漫散取向的晶粒间也形成较多的{111}/{111}近奇异晶界,这是导致经-196 ℃深冷轧制及再结晶的样品中{111}/{111}近奇异晶界比例较高的主要原因。

关键词 高纯Al深冷轧制近奇异晶界晶界界面匹配    
Abstract

Recent advancements in grain boundary engineering have revealed that the {111}/{111} near singular boundary (NSB) exhibits superior resistance to corrosion attacks than the random boundary in aluminum and its alloys. Thus, understanding the influential factors and formation mechanisms of the {111}/{111} NSB, as well as regulating such boundaries, is crucial for enhancing the resistance performance of aluminum and its alloys against intergranular corrosion attacks. To intrinsically comprehend the formation mechanism of the {111}/{111} NSB in aluminum alloys, this study used high purity aluminum (99.99%) as the experimental material. Initially, the starting samples were synthesized through multidirectional forging at room temperature (25 oC), followed by recrystallization annealing at 370 oC. The as-synthesized starting samples exhibited uniform microstructures with an average grain size of 20 μm and random grain orientations. Subsequently, two parallel starting samples were rolled at 25 oC and at the cryogenic temperature (-196 oC), respectively, with an 80% thickness reduction, followed by immediate recrystallization annealing at 370 oC for 30 min. Later, a quantitative grain boundary inter-connection characterization method based on EBSD and five parameter analysis was employed to statistically analyze the grain boundary character distributions within the samples. The results revealed that the cryo-rolled and recrystallized sample featured a higher proportion of the {111}/{111} NSB compared to the 25 oC-rolled and recrystallized sample. Specifically, the {111}/{111} NSB fraction in the former reached 6.0%, 2.22 times that in the latter. XRD analysis, hardness testing, and EBSD measurements revealed the development of a strong {011}<111¯> deformation texture in the samples rolled at 25 oC or the cryogenic temperature. In particular, cryo-rolling was found to impede dynamic recovery; hence, the sample rolled at this temperature featured higher levels of residual compression stress, increased grain fragmentation, and higher stored energy compared to the sample rolled at 25 oC. Owing to the higher driving force and more active {011}<011¯>-oriented growth, the cryo-rolled sample formed larger grains and stronger {011}<011¯> recrystallization textures during the subsequent recrystallization annealing. Statistical analysis based on grain boundary tracing demonstrated that the grain boundaries between {011}<011¯>-oriented grains and other oriented grains contained higher proportions of the {111}/{111} NSB compared to the grain boundaries between two randomly oriented grains. Moreover, boundaries between the {011}<011¯>- oriented grains and their diffusive orientations featured notably high proportions of the {111}/{111} NSB. This explains the higher content of the {111}/{111} NSB observed in the cryo-rolled and recrystallized sample than that in the 25 oC-rolled and recrystallized sample.

Key wordshigh purity aluminum    cryo-rolling    near singular boundary    grain boundary inter-connection
收稿日期: 2024-01-30     
ZTFLH:  TG146.2  
基金资助:国家自然科学基金项目(51971063);福建省自然科学基金项目(2021J011076)
通讯作者: 王卫国,wang_weiguo@vip.163.com,主要从事金属和无机非金属材料晶界工程研究
Corresponding author: WANG Weiguo, professor, Tel: (0591)22863515, E-mail: wang_weiguo@vip.163.com
作者简介: 李振想,男,1998年生,硕士生

Sample

Rolling temperature

oC

Thickness

reduction

%

Annealing

Sample

Rolling temperature

oC

Thickness

reduction

%

Annealing

A2580-A1-19680-
B2580370 oC, 6 minB1-19680370 oC, 6 min
C2580370 oC, 12 minC1-19680370 oC, 12 min
D2580370 oC, 18 minD1-19680370 oC, 18 min
E2580370 oC, 24 minE1-19680370 oC, 24 min
F2580370 oC, 30 minF1-19680370 oC, 30 min
表1  高纯Al样品编号及其加工状态
图1  F和F1样品的显微组织取向成像显微(OIM)图、晶界网络和取向差分布图
SampleRotation axisGB numberNumber fraction / %Length fraction / %
F<111>33836.706.97
<112>591311.7011.64
<122>812616.0016.23
F1<111>39647.507.44
<112>613311.7011.74
<122>906517.3017.22
表2  F和F1样品中取向差转轴为<111>、<112>和<122>的晶界数量及比例统计
图2  F和F1样品的固定转轴晶界取向差分布图
图3  F样品中存在{111}/{111}-近奇异晶界(NSB)的各组晶界的晶界面分布(GBPD)图(投影在(001)内)
图4  F1样品中存在{111}/{111}-NSB的各组晶界的GBPD图(投影在(001)内)
Sample[uvw]/θ'Pi / %MiWi / (º)Fi / %F = ∑Fi / %
F[111]/20º0.301.701.550.162.70
[111]/25º0.361.702.140.19
[111]/30º0.392.151.890.21
[111]/55º1.101.482.370.56
[112]/30º1.011.392.420.52
[122]/20º0.861.572.370.44
[122]/30º1.211.241.930.62
F1[111]/15º0.301.421.930.166.00
[111]/25º0.342.702.070.18
[111]/30º0.441.642.360.22
[111]/35º0.481.721.990.25
[111]/40º0.631.481.610.33
[111]/45º0.731.601.960.39
[111]/50º0.981.901.900.52
[111]/55º1.201.572.020.61
[112]/25º0.871.312.220.44
[122]/20º0.931.552.510.48
[122]/25º0.831.562.230.43
[122]/30º1.141.372.170.60
[122]/35º1.201.582.210.62
[122]/40º1.471.251.920.77
表3  F和F1样品的{111}/{111}-NSB相关数据统计
图5  A和A1样品的轧面(A-ND和A1-ND)、横切面(A-RD和A1-RD)及纯Al粉末样品(Powder)的XRD谱
图6  轧制样品及轧制后370 ℃退火样品的{022}XRD谱
图7  轧制样品及轧制后370 ℃退火样品沿轧板厚度方向的压应力
图8  轧制样品及轧制后370 ℃退火样品的Vickers硬度
图9  经室温和深冷轧制后再经370 ℃退火不同时间各样品的平均晶粒尺寸
图10  经室温和深冷轧制后再经370 ℃退火不同时间各样品的ODF截面图
RollingGrainNumber ofNumber ofNumber of NSBPercentage of
temperatureorientationgrainboundaryNSB / %
RT{100}<001>107334.1
{011}<011¯>106446.3
{111}<011¯>107434.0
CT{100}<001>107645.3
{011}<011¯>106369.5
{111}<011¯>107022.9
表4  随机选取3种不同取向的各10个晶粒所关联晶界的特征统计
图11  {011}<011¯>取向晶粒与其他取向晶粒间形成{111}/{111}-NSB的显微组织OIM图和{111}重叠极图晶界迹线分析
图12  {011}<011¯>取向晶粒与其漫散取向晶粒间形成{111}/{111}-NSB的显微组织OIM图和{111}重叠极图晶界迹线分析
Grain boundaryOrientation of grains G, H, and IOrientation of grains J, K, and L

Misorientation

[uvw]/θ'

Euler angle

(φ1, Ф, φ2)

Miller indexed

Euler angle

(φ1, Ф, φ2)

Miller indexed
GBGJG: 1°, 90°, 39°{011}<011¯>J: 212°, 21°, 27°{126}<2¯41¯>[11¯1]/41.4°
GBHKH: 359°, 91°, 42°{011}<011¯>K: 226°, 33°, 57°{326}<2156¯>[11¯1]/35.8°
GBILI: 356°, 86°, 45°{011}<011¯>L: 59°, 32°, 69°{314}<04¯1>[11¯1]/45.8°
表5  {011}<011¯>取向晶粒与其他取向晶粒间形成{111}/{111}-NSB的相关信息(对应图11)
图13  {011}<011¯>取向晶粒(P1和P2)与{011}<011¯>漫散取向晶粒M及其他取向晶粒N之间形成{111}/{111}-NSB的晶胞示意图
Orientation of grains P1 and P2Orientation of grains M and N

Misorientation

[uvw]/θ'

Euler angle

(φ1, Ф, φ2)

Miller indexed

Euler angle

(φ1, Ф, φ2)

Miller indexed
P1: -4.6°, 89°, 43°{011}<011¯>M: 11°, 88°,5 5°{320}<34¯1>[111]/19.9°
P2: 0°, 90°, 46°{011}<011¯>N: 55°, 32°, 45°{112}<02¯1>[11¯1/29.5°
  
Grain boundaryOrientation of grains A, B, and COrientation of grains D, E, and F

Misorientation

[uvw]/θ'

Euler angle

(φ1, Ф, φ2)

Miller indexed

Euler angle

(φ1, Ф, φ2)

Miller indexed
GBADA: 357°, 89°, 39°{011}<011¯>D: 10°, 89°, 46°{110}<44¯1>[111]/15.2°
GBBEB: 356°, 92°, 39°{011}<011¯>E: 19°, 90°, 57°{320}<69¯4>[11¯1]/28.8°
GBCFC: 356°, 87°, 45°{011}<011¯>F: 12°, 86°, 56°{320}<69¯2>[111]/20.3°
表6  {011}<011¯>取向晶粒与{011}<011¯>漫散取向晶粒形成{111}/{111}-NSB的相关信息(对应图12)
[1] Deng Y L, Zhang X M. Development of aluminium and aluminium alloy [J]. Chin. J. Nonferrous Met., 2019, 29: 2115
[1] 邓运来, 张新明. 铝及铝合金材料进展 [J]. 中国有色金属学报, 2019, 29: 2115
[2] Hong T J, Dong F L, Ding F J, et al. Application of aluminum alloy in automotive lightweight [J]. Hot Work. Technol., 2020, 49(4): 1
[2] 洪腾蛟, 董福龙, 丁凤娟 等. 铝合金在汽车轻量化领域的应用研究 [J]. 热加工工艺, 2020, 49(4): 1
[3] Liang G, Zhu S, Wang W Y, et al. Research status and development trend of aluminum alloy anticorrosion technology [J]. Mater. Rev., 2020, 34(): 429
[3] 梁 广, 朱 胜, 王文宇 等. 铝合金腐蚀防护技术研究现状及发展趋势 [J]. 材料导报, 2020, 34(): 429
[4] He T, Shi W, Xiang S, et al. Influence of aging on corrosion behaviour of the 6061 cast aluminium alloy [J]. Materials (Basel), 2021, 14: 1821
[5] Liu Y R, Pan Q L, Li H, et al. Revealing the evolution of microstructure, mechanical property and corrosion behavior of 7A46 aluminum alloy with different ageing treatment [J]. J. Alloys Compd., 2019, 792: 32
[6] Aust K T. Grain boundary engineering [J]. Can. Metall. Quart., 1994, 33: 265
[7] Wang W G, Zhou B X, Rohrer G S, et al. Textures and grain boundary character distributions in a cold rolled and annealed Pb-Ca based alloy [J]. Mater. Sci. Eng., 2010, A527: 3695
[8] Liu Z Q, Wang W G. Study on Σ3 boundaries in an cold rolled and recrystallized Al-Cu alloy [J]. J. Chin. Electron Microsc. Soc., 2018, 37: 232
[8] 刘智强, 王卫国. 冷轧变形Al-Cu合金再结晶Σ3晶界研究 [J]. 电子显微学报, 2018, 37: 232
[9] Wang W G, Cai C H, Rohrer G S, et al. Grain boundary inter-connections in polycrystalline aluminum with random orientation [J]. Mater. Charact., 2018, 144: 411
[10] Yang X M, Wang W G, Gu X F. The near singular boundaries in BCC iron [J]. Philos. Mag., 2022, 102: 440
[11] Wang W G, Du A H, Yang X M, et al. Quantitative determination of grain boundary inter-connections [P]. Chin Pat, CN2020111-73146.8, 2021
[11] 王卫国, 杜阿华, 杨先明 等. 晶界界面匹配定量表征方法 [P]. 中国专利, CN202011173146.8, 2021)
[12] Randle V, Rohrer G S, Hu Y. Five-parameter grain boundary analysis of a titanium alloy before and after low-temperature annealing [J]. Scr. Mater., 2008, 58: 183
[13] Zhang W Z. Application of the O-lattice model to the calculation of the interfacial dislocations [J]. Acta Metall. Sin., 2002, 38: 785
[13] 张文征. O点阵模型及其在界面位错计算中的应用 [J]. 金属学报, 2002, 38: 785
[14] Du A H, Wang W G, Gu X F, et al. The dependence of precipitate morphology on the grain boundary types in an aged Al-Cu binary alloy [J]. J. Mater. Sci., 2021, 56: 781
[15] Wang Z P, Wang W G, Rohrer G S, et al. {111}/{111} Near singular boundaries in a Al-Zn-Mg-Cu Alloy recrystallized after rolling at different temperatures [J]. Acta Metall. Sin., 2023, 59: 947
[15] 王宗谱, 王卫国, Rohrer G S 等. 不同温度轧制Al-Zn-Mg-Cu合金再结晶后的{111}/{111}近奇异晶界 [J]. 金属学报, 2023, 59: 947
[16] Takayama A, Yang X, Miura H, et al. Continuous static recrystallization in ultrafine-grained copper processed by multi-directional forging [J]. Mater. Sci. Eng., 2008, A478: 221
[17] Feng X Z, Wang W G, Rohrer G S, et al. Effects of grain growth on the {111}/{111} near singular boundaries in high purity aluminum [J]. Acta Metall. Sin., 2024, 60: 80
[17] 冯小铮, 王卫国, Rohrer G S 等. 晶粒长大对高纯Al{111}/{111}近奇异晶界的影响 [J]. 金属学报, 2024, 60: 80
[18] Tong F, Wang W G, Rohrer G S, et al. Effect of pre-deformation temperature on formation of {111}/{111} near singular boundaries in Al-Mg alloy during subsequent recrystallization [J]. Trans. Mater. Heat Treat., 2023, 44(5): 47
[18] 童 芳, 王卫国, Rohrer G S 等. 预变形温度对Al-Mg合金再结晶{111}/{111}近奇异晶界的影响 [J]. 材料热处理学报, 2023, 44(5): 47
[19] Lee Y B, Shin D H, Park K T, et al. Effect of annealing temperature on microstructures and mechanical properties of a 5083 Al alloy deformed at cryogenic temperature [J]. Scr. Mater., 2004, 51: 355
[20] Chen D, Li W X. Cryogenic treatment of Al and Al alloys [J]. Chin. J. Nonferrous Met., 2000, 10: 891
[20] 陈 鼎, 黎文献. 铝和铝合金的深冷处理 [J]. 中国有色金属学报, 2000, 10: 891
[21] Barron R F. Cryogenic treatment of metals to improve wear resistance [J]. Cryogenics, 1982, 22: 409
[22] Koneshlou M, Asl K M, Khomamizadeh F. Effect of cryogenic treatment on microstructure, mechanical and wear behaviors of AISI H13 hot work tool steel [J]. Cryogenics, 2011, 51: 55
[23] Molinari A, Pellizzari M, Gialanella S, et al. Effect of deep cryogenic treatment on the mechanical properties of tool steels [J]. J. Mater. Process. Technol., 2001, 118: 350
[24] Podgornik B, Paulin I, Zajec B, et al. Deep cryogenic treatment of tool steels [J]. J. Mater. Process. Technol., 2016, 229: 398
[25] Shi J T, Zuo J R, Zhang J S. Microstructure and mechanical properties of 5052 Al alloy by cryogenic rolling [J]. Mater. Sci. Forum., 2020, 993: 86
[26] Wolf D. Structure-energy correlation for grain boundaries in F.C.C. metals—I. Boundaries on the (111) and (100) planes [J]. Acta Metall., 1989, 37: 1983
[27] Wright S I, Larsen R J. Extracting twins from orientation imaging microscopy scan data [J]. J. Microsc., 2002, 205: 245
[28] Wang W G, Lin C, Li G H, et al. Preferred orientation of grain boundary plane in recrystallized high purity aluminum [J]. Sci. Sin. Technol., 2014, 44: 1295
[29] Krishna N N, Ashfaq M, Susila P, et al. Mechanical anisotropy and microstructural changes during cryorolling of Al-Mg-Si alloy [J]. Mater. Charact., 2015, 107: 302
[30] Krishna N N, Tejas R, Sivaprasad K, et al. Study on cryorolled Al-Cu alloy using X-ray diffraction line profile analysis and evaluation of strengthening mechanisms [J]. Mater, Des., 2013, 52: 785
[31] Hou L G, Liu M L, Wang X D, et al. Cryogenic processing high-strength 7050 aluminum alloy and controlling of the microstructures and mechanical properties [J]. Acta Metall. Sin., 2017, 53: 1075
[31] 侯陇刚, 刘明荔, 王新东 等. 高强7050铝合金超低温大变形加工与组织、性能调控 [J]. 金属学报, 2017, 53: 1075
[32] Rangaraju N, Raghuram T, Krishna B V, et al. Effect of cryo-rolling and annealing on microstructure and properties of commercially pure aluminium [J]. Mater. Sci. Eng., 2005, A398: 246
[33] Xiong Y, He T T, Guo Z Q, et al. Effect of severe deformation under different temperatures and annealing on microstructure of commercial pure aluminum [J]. Trans. Mater. Heat Treat., 2011, 32(9): 63
[33] 熊 毅, 贺甜甜, 郭志强 等. 不同温度重度变形及退火对工业纯铝组织的影响 [J]. 材料热处理学报, 2011, 32(9): 63
[34] Barrett C S. Recrystallization texture in aluminum after compression [J]. Trans. Aime, 1940, 137: 128
[35] Engler O, Vatne H E, Nes E. The roles of oriented nucleation and oriented growth on recrystallization textures in commercial purity aluminium [J]. Mater. Sci. Eng., 1996, A205: 187
[1] 刘光辉, 王卫国, Rohrer Gregory S, 陈松, 林燕, 童芳, 冯小铮, 周邦新. 高温压缩变形Al-Zn-Mg-Cu合金动态再结晶后的{111}/{111}近奇异晶界[J]. 金属学报, 2024, 60(9): 1165-1178.
[2] 冯小铮, 王卫国, Gregory S. Rohrer, 陈松, 洪丽华, 林燕, 王宗谱, 周邦新. 晶粒长大对高纯Al {111}/{111}近奇异晶界的影响[J]. 金属学报, 2024, 60(1): 80-94.
[3] 王宗谱, 王卫国, Rohrer Gregory S, 陈松, 洪丽华, 林燕, 冯小铮, 任帅, 周邦新. 不同温度轧制Al-Zn-Mg-Cu合金再结晶后的{111}/{111}近奇异晶界[J]. 金属学报, 2023, 59(7): 947-960.
[4] 陈吉湘,王卫国,林燕,林琛,王乾廷,戴品强. 等径角挤压和单向轧制高纯Al再结晶晶界面的取向分布*[J]. 金属学报, 2016, 52(4): 473-483.