高 γ′相含量GH4151变形高温合金铸态组织与开裂敏感性分析
钟佳, 王法, 江河, 姚志浩, 董建新()
北京科技大学 材料科学与工程学院 北京 100083
Analyses of As-Cast Microstructure and Cracking Sensitivity of GH4151 Wrought Superalloy with High γ′ Phase Content
ZHONG Jia, WANG Fa, JIANG He, YAO Zhihao, DONG Jianxin()
School of Materials Science and Engineering, University of Science and Technology Beijing, Beijing 100083, China
引用本文:

钟佳, 王法, 江河, 姚志浩, 董建新. 高 γ′相含量GH4151变形高温合金铸态组织与开裂敏感性分析[J]. 金属学报, 2025, 61(11): 1653-1663.
Jia ZHONG, Fa WANG, He JIANG, Zhihao YAO, Jianxin DONG. Analyses of As-Cast Microstructure and Cracking Sensitivity of GH4151 Wrought Superalloy with High γ′ Phase Content[J]. Acta Metall Sin, 2025, 61(11): 1653-1663.

全文: PDF(3787 KB)   HTML
摘要: 

GH4151合金化程度高,凝固偏析严重,析出相多且复杂,易造成合金开裂。本工作采用OM、SEM、DSC、萃取相分析、XRD、热压缩模拟和热力学计算方法研究了GH4151合金铸态组织与开裂敏感性,分析了GH4151合金的元素偏析、铸态组织、相析出行为以及开裂特征。结果表明,GH4151合金中Nb元素偏析严重,偏析系数高达2.3。元素偏析促进铸锭枝晶间析出大量γ′相、约0.176%的Laves相 (质量分数)、0.289%的MC碳化物、γ/γ′共晶相和η相等。枝晶间析出尺寸较为粗大且形貌不规则的复杂析出相,析出相与基体相界面处易萌生裂纹并沿着界面处扩展。同时,γ′相含量高达41.177%,高γ′相含量使得GH4151合金的热导率降低,导致合金铸锭在冷却过程中更容易积累热应力。凝固偏析、不规则析出相与热应力易积累的共同作用,导致GH4151合金铸锭呈现易开裂敏感性。

关键词 : GH4151变形高温合金,  铸态组织,  元素偏析,  裂纹分析    
Abstract:

Nickel-based superalloys, known for their excellent high-temperature mechanical characteristics and structural stability, are extensively utilized in critical high-temperature components of gas turbine engines, including combustion chambers, turbine blades, and turbine disks. With the development of aeronautical technology, the required maximum operating temperature of turbine disks is 800 oC and above. To meet such high-temperature application requirements, China designed GH4151, a new type of nickel-based wrought superalloy that contains precipitation strengthening elements such as Al, Nb, and Ti along with solid solution strengthening elements such as Cr, Co, Mo, and W. The weight ratio of the solid solution strengthening elements was 34% and that of the precipitation strengthening elements was 10%. Due to the high alloying degree of GH4151 wrought superalloy, its smelting process often results in solute distribution and element segregation between liquid and solid phases, which can lead to the precipitation of numerous harmful phases during solidification, causing cracks in the ingot. Subsequent processing becomes impossible once cracks appear. To study the cast microstructure complexity and its correlation with ingot cracking, the elemental segregation, cast microstructure, phase precipitation behavior, and cracking characteristics of GH4151 wrought superalloy were analyzed by OM, SEM, DSC, extraction phase analysis, XRD, hot compression simulation, and thermodynamic calculations. The results indicated that Nb segregation in GH4151 ingots was severe, with a segregation coefficient as high as 2.3. Elemental segregation in the alloy led to the precipitation of various phases, including massive γ′ phases, Laves phases, MC carbides, γ/γ′ eutectic phases, and η phases. The γ′ phase, Laves phase, and MC carbide structures are Ni2.42Co0.40Cr0.10Mo0.04W0.03Ti0.26Al0.59Nb0.12V0.03, (Co0.241Cr0.205Ni0.554)2(Nb0.309Mo0.242Ti0.346W0.102), and (Ti0.333Nb0.521Mo0.100W0.028V0.019)C, respectively. Due to elemental segregation, numerous precipitated phases with coarse sizes and irregular morphologies formed during solidification. The GH4151 ingot was highly susceptible to cracking, with potential crack formation at the interface of complex precipitates between dendrites, namely Laves phases, γ/γ′ eutectic phases, MC carbides, η phases, and the matrix. A high γ′ phase content of 41.177% in GH4151 reduced its thermal conductivity and increased the likelihood of thermal stress accumulation during cooling, ultimately leading to increased cracking sensitivity in the alloy ingot due to a combination of solidification segregation and thermal stress accumulation.

Key words: GH4151 wrought superalloy    as-cast microstructure    element segregation    crack analysis
收稿日期: 2024-01-29     
ZTFLH:  TG115.23  
基金资助:国家科技重大专项项目(J2019-VI-0021-0137)
通讯作者: 董建新,jxdong@ustb.edu.cn,主要从事高温合金的研发工作
Corresponding author: DONG Jianxin, professor, Tel: (010)62332884, E-mail: jxdong@ustb.edu.cn
作者简介: 钟 佳,女,1998年生,博士生
图1  直径410 mm的GH4151合金自耗锭不同区域枝晶形貌的OM像
RegionPrimary dendrite arm spacing / μmSecondary dendrite arm spacing / μmSegregation coefficient
AlTiVCrCoNbMoW
Edge146.982.60.81.01.11.01.01.81.31.1
1/2 radius381.7112.70.91.30.80.90.92.31.21.0
Center496.9133.00.91.60.71.01.02.31.30.6
表1  GH4151合金自耗锭不同区域的枝晶臂间距及元素偏析系数
图2  基于JMatPro软件得到的GH4151合金热力学计算结果
图3  直径410 mm的GH4151合金自耗锭铸态组织的SEM像
PhaseCAlTiVCrCoNiNbMoW
Laves–1.21.60.421.122.225.312.213.72.3
η–6.58.1–3.612.661.06.51.20.5
γ/γ′ eutectic–9.77.3–3.012.763.13.11.00.1
MC56.30.110.80.30.30.41.628.90.80.5
表2  铸态GH4151合金枝晶间各析出相的化学成分 (mass fraction / %)
图4  直径410 mm的GH4151合金自耗锭不同区域γ′相的SEM像
图5  GH4151合金萃取析出相粉末的XRD谱
PhaseNiCNbTiAlCoCrMoWVTotal
γ′26.282-2.1252.2992.9454.3410.9890.7401.1820.274041.177
Laves0.055-0.0260.015-0.0240.0180.0210.017-0.176
MC-0.0380.1520.050---0.0300.0160.00300.289
表3  直径410 mm的GH4151合金自耗锭中各物相的成分及占比 (mass fraction / %)
图6  GH4151合金在10 ℃/min速率下的升温和降温DSC曲线
图7  基于JMatPro软件计算得到的GH4151合金凝固路径

Phase

JMatPro valueHeating temperature pointCooling temperature point
Liquid132613251315
Solid126712491308
MC129512901254
η1160-1163
γ′117511501112, 1163
γ/γ′-11501130
Laves1095-1090
表4  GH4151合金凝固期间的相变点温度 (oC)
图8  GH4151合金凝固过程示意图
图9  直径410 mm的GH4151合金自耗锭在1120 ℃等温热压缩实验后的宏观形貌及不同相界面的SEM像(1 s-1应变速率、30%变形量)
图10  直径 410 mm的GH4151合金自耗锭裂纹区组织形貌的SEM像
图11  基于JMatPro软件计算得到的不同合金热导率随温度变化的曲线
[1] Wang F. The influence of characteristics due to high-content γ′ on microstructures and properties of difficult-to-deform GH4151 alloy and the exploration of alloys with higher service temperature [D]. Beijing: University of Science and Technology Beijing, 2023
[1] 王 法. 高含量γ′特性对难变形GH4151合金组织性能影响及更高使用温度合金探索 [D]. 北京: 北京科技大学, 2023
[2] Zhang J, Wang L, Xie G, et al. Recent progress in research and development of nickel-based single crystal superalloys [J]. Acta Metall. Sin., 2023, 59: 1109
[2] 张 健, 王 莉, 谢 光 等. 镍基单晶高温合金的研发进展 [J]. 金属学报, 2023, 59: 1109
[3] Yin B, Xie G, Lou L H, et al. Abnormal increase of TCP phase during heat treatment in a Ni-based single crystal superalloy [J]. Scr. Mater., 2019, 173: 1
[4] Xu Z Q, Yang S F, Zhao P, et al. Phase precipitation and segregation behavior of nickel-based superalloy GH4151 [J]. J. Iron Steel Res., 2022, 34: 588
[4] 徐志强, 杨树峰, 赵 朋 等. 镍基高温合金GH4151的偏析及相析出行为 [J]. 钢铁研究学报, 2022, 34: 588
[5] Li X X, Jia C L, Zhang Y, et al. Cracking mechanism in as-cast GH4151 superalloy ingot with high γ′ phase content [J]. Trans. Nonferrous Met. Soc. China, 2020, 30: 2697
[6] Lv S M, Chen J B, He X B, et al. Investigation on sub-solvus recrystallization mechanisms in an advanced γ-γ′ nickel-based superalloy GH4151 [J]. Materials, 2020, 13: 4553
[7] Bi Z N, Qu J L, Du J H, et al. Microstructure characteristics and thermodynamic calculation of equilibrium precipitated phases in a new difficult-to-deform superalloy эк151 [J]. Rare Met. Mater. Eng., 2013, 42: 919
[7] 毕中南, 曲敬龙, 杜金辉 等. 新型难变形高温合金эк151的组织特征及平衡析出相热力学计算 [J]. 稀有金属材料与工程, 2013, 42: 919
[8] Bi Z N, Qu J L, Du J H, et al. Segregation behavior and investigation on homogenization for a new difficult-to-deform superalloy ЭК151 ingot [J]. J. Iron Steel Res., 2011, 23(suppl.2): 263
[8] 毕中南, 曲敬龙, 杜金辉 等. 新型难变形高温合金ЭК151的偏析行为及均匀化工艺研究 [J]. 钢铁研究学报, 2011, 23(): 263
[9] Zhao Z, Dong J X, Zhang M C, et al. Microstructure and susceptibility to hot tearing of K424 nickel-based superalloys for turbocharger turbine wheels [J]. Chin. J. Eng., 2016, 38: 1429
[9] 赵 展, 董建新, 张麦仓 等. 增压涡轮用K424高温合金组织特征及热裂倾向性 [J]. 工程科学学报, 2016, 38: 1429
[10] Zhao Z, Dong J X, Zhang M C, et al. Solidification characteristics and microstructures evolution of Ni-based superalloy K424 with different solidification cooling rates [J]. Chin. J. Eng., 2018, 40: 1332
[10] 赵 展, 董建新, 张麦仓 等. K424高温合金凝固特征及冷却速度对其影响规律 [J]. 工程科学学报, 2018, 40: 1332
[11] Zhao Z. Influences and control of microstructures and process on hot-tearing for superalloy turbocharger turbine wheels [D]. Beijing: University of Science and Technology Beijing, 2020
[11] 赵 展. 增压涡轮用高温合金组织和工艺对热裂的影响与控制 [D]. 北京: 北京科技大学, 2020
[12] Xu J J, Lin X, Guo P F, et al. The initiation and propagation mechanism of the overlapping zone cracking during laser solid forming of IN-738LC superalloy [J]. J. Alloys Compd., 2018, 749: 859
[13] Zhou Y Z, Volek A, Singer R F. Effect of grain boundary characteristics on hot tearing in directional solidification of superalloys [J]. J. Mater. Res., 2006, 21: 2361
[14] Fojt-Dymara G, Opiela M, Borek W. Susceptibility of high-manganese steel to high-temperature cracking [J]. Materials, 2022, 15: 8198
[15] Jia L, Cui H, Yang S F, et al. The cracking behavior of the new Ni-based superalloy GH4151 in the triple melting process [J]. J. Mater. Res. Technol., 2023, 25: 2368
[16] Lv S M, Jia C L, He X B, et al. Superplastic deformation and dynamic recrystallization of a novel disc superalloy GH4151 [J]. Materials, 2019, 12: 3667
[17] Tan Y G. Investigation of solidification and high-temperature deformation behavior of Ni-base alloy ЭК151 [D]. Hefei: University of Science and Technology of China, 2019
[17] 谭远过. 新型镍基高温合金ЭК151凝固偏析及高温变形行为研究 [D]. 合肥: 中国科学技术大学, 2019
[18] Tan Y G, Liu F, Zhang A W, et al. Element segregation and solidification behavior of a Nb, Ti, Al Co-strengthened superalloy ЭК151 [J]. Acta Metall. Sin. (Engl. Lett.), 2019, 32: 1298
[19] Kong D C, Dong C F, Ni X Q, et al. High-throughput fabrication of nickel-based alloys with different Nb contents via a dual-feed additive manufacturing system: Effect of Nb content on microstructural and mechanical properties [J]. J. Alloys Compd., 2019, 785: 826
[20] Jiang H, Nai Q L, Xu C, et al. Sensitive temperature and reason of rapid fatigue crack propagation in nickel-based superalloy [J]. Acta Metall. Sin., 2023, 59: 1190
[20] 江 河, 佴启亮, 徐 超 等. 镍基高温合金疲劳裂纹急速扩展敏感温度及成因 [J]. 金属学报, 2023, 59: 1190
[21] Li Y S, Dong Y W, Jiang Z H, et al. Study on microsegregation and homogenization process of a novel nickel-based wrought superalloy [J]. J. Mater. Res. Technol., 2022, 19: 3366
[22] Bi Z N, Qin H L, Dong Z G, et al. Residual stress evolution and its mechanism during the manufacture of superalloy disk forgings [J]. Acta Metall. Sin., 2019, 55: 1160
[22] 毕中南, 秦海龙, 董志国 等. 高温合金盘锻件制备过程残余应力的演化规律及机制 [J]. 金属学报, 2019, 55: 1160
[23] Zhou H, Wang P, Lu S P. Effect of grain boundary morphology and MC on plastic deformation behavior of NiCrFe weld metal: Crystal plasticity finite element analysis [J]. Chin. J. Mater. Res., 2019, 33: 801
[23] 周 辉, 王 培, 陆善平. NiCrFe焊缝金属的晶界形貌和晶界MC碳化物对局部变形行为的影响 [J]. 材料研究学报, 2019, 33: 801
[24] Wu Y S. Effect of phosphorus on the deformation behavior of GH984G alloy [D]. Hefei: University of Science and Technology of China, 2020
[24] 吴云胜. 磷含量对GH984G合金变形行为的影响 [D]. 合肥: 中国科学技术大学, 2020
[25] Lu N N, Guo Y M, Yang S L, et al. Formation mechanisms of hot cracks in laser additive repairing single crystal superalloys [J]. Acta Metall. Sin., 2023, 59: 1243
[25] 卢楠楠, 郭以沫, 杨树林 等. 激光增材修复单晶高温合金的热裂纹形成机制 [J]. 金属学报, 2023, 59: 1243
[26] Wang X Q, Gong X B, Chou K. Review on powder-bed laser additive manufacturing of Inconel 718 parts [J]. Proc. Inst. Mech. Eng., 2017, 231B: 1890
[27] Chen Y, Zhang K, Huang J, et al. Characterization of heat affected zone liquation cracking in laser additive manufacturing of Inconel 718 [J]. Mater. Des., 2016, 90: 586
[28] Wang T, Wan Z P, Li Z, et al. Effect of heat treatment parameters on microstructure and hot workability of as-cast fine grain ingot of GH4720Li alloy [J]. Acta Metall. Sin., 2020, 56: 182
[28] 王 涛, 万志鹏, 李 钊 等. 热处理工艺对GH4720Li合金细晶铸锭组织与热加工性能的影响 [J]. 金属学报, 2020, 56: 182
[29] Wang D, Liu Z, Wang J G, et al. Study on microstructure and properties of shaped ring parts for super alloy GH4738 [J]. Forg. Stamp. Technol., 2020, 45(5): 128
[29] 王 丹, 刘 智, 王建国 等. GH4738高温合金异形环件组织与性能研究 [J]. 锻压技术, 2020, 45(5): 128
[30] Yan X F, Dong J X, Shi Z X, et al. Solidification and segregation behavior of nickel-based superalloy GH4282 [J]. Rare Met. Mater. Eng., 2019, 48: 3183
[30] 颜晓峰, 董建新, 石照夏 等. 镍基高温合金GH4282的凝固和偏析行为 [J]. 稀有金属材料与工程, 2019, 48: 3183
[1] 张勇, 李鑫旭, 韦康, 韦建环, 王涛, 贾崇林, 李钊, 马宗青. 三联熔炼GH4169合金大规格铸锭与棒材元素偏析行为[J]. 金属学报, 2020, 56(8): 1123-1132.
[2] 罗银屏, 周亦胄, 刘金来. Ru和Cr在一种无Re镍基单晶高温合金凝固过程中的作用[J]. 金属学报, 2014, 50(9): 1025-1030.
[3] 刘静 罗兴宏 胡小强 刘实. Ti和Nb微合金化对超纯11%Cr铁素体不锈钢组织的影响[J]. 金属学报, 2011, 47(6): 688-696.
[4] 刘雅晶; 李玉清; 谢锡善; J.H.Tundermann; 董建新; 郭晓倬 . Al, Ti和Nb对Fe-Ni-Cr-Co-Nb-Ti-Al合金铸态组织的影响[J]. 金属学报, 1999, 35(10): 1036-1042 .
[5] 丁培道;石功奇;周守则. Fe-Mo-C合金铸态组织的电镜观察[J]. 金属学报, 1990, 26(6): 15-18.
[6] 邱一鸣;朱耀霄. 镍基铸造高温合金中合金元素的偏析规律[J]. 金属学报, 1989, 25(1): 78-80.