Please wait a minute...
金属学报  2022, Vol. 58 Issue (10): 1236-1252    DOI: 10.11900/0412.1961.2022.00175
  综述 本期目录 | 过刊浏览 |
连铸结晶器内高温熔体多相流模型化研究进展
刘中秋1,2, 李宝宽1(), 肖丽俊2, 干勇2
1.东北大学 冶金学院 沈阳 110819
2.钢铁研究总院 北京 100081
Modeling Progress of High-Temperature Melt Multiphase Flow in Continuous Casting Mold
LIU Zhongqiu1,2, LI Baokuan1(), XIAO Lijun2, GAN Yong2
1.School of Metallurgy, Northeastern University, Shenyang 110819, China
2.Central Iron and Steel Research Institute, Beijing 100081, China
引用本文:

刘中秋, 李宝宽, 肖丽俊, 干勇. 连铸结晶器内高温熔体多相流模型化研究进展[J]. 金属学报, 2022, 58(10): 1236-1252.
Zhongqiu LIU, Baokuan LI, Lijun XIAO, Yong GAN. Modeling Progress of High-Temperature Melt Multiphase Flow in Continuous Casting Mold[J]. Acta Metall Sin, 2022, 58(10): 1236-1252.

全文: PDF(3998 KB)   HTML
摘要: 

连铸结晶器内高温熔体多相流的运动状态强烈地影响高品质钢的洁净化、均匀化和精细化。该高温熔体多相流为非稳态湍流,同时耦合传热、传质、相变、反应、电磁力等诸多过程,形成了十分复杂的非稳态、非线性、非平衡多物理场,很难通过现场测试对其内部的各种物理量进行在线测量。在确保流动和凝固过程相似的情况下,开展物理模拟实验以及对其多尺度传输现象的数值模拟,已成为阐述连铸坯各类缺陷形成机理的首选。然而,与传统流体力学问题相比,冶金高温熔体多相流的突出特点是物性变化大、本构关系式复杂、相界面影响因素多及边界物理量梯度大等,且连铸结晶器内多物理场存在连续相大界面变形、离散相颗粒输运以及连续相-离散相转变等复杂多变的多尺度界面现象,以及多尺度的湍流涡结构,这些都给高温熔体多相流模型化研究带来极大困难。相比于单相流,多相流具有相界面拓扑形状变化的特征,本文从离散流界面尺度分布性、混合流界面跨尺度性、凝固界面多尺度性、以及湍流在揭示多尺度相界面结构中的作用等4方面回顾了连铸结晶器内高温熔体多相流模型化的研究进展,并展望了未来可能的研究方向。

关键词 : 连铸结晶器,  高温熔体,  多相流,  多尺度,  模型化    
Abstract:

The cleanliness, homogenization, and refinement of the high-quality steel are highly dependent on the high-temperature melt multiphase flow in the continuous casting mold. The high-temperature melt multiphase flow is unsteady-state turbulence that is coupled with heat transfer, mass transfer, phase change, chemical reaction, and electromagnetic effect, forming an extremely complex, unsteady, nonlinear, and nonequilibrium multiphysical fields, where various physical quantities are nearly impossible to on-line measure through on-site testing. With the similarity of flow and solidification processes ensured, both the physical experiment and the numerical simulation of multiscale transport phenomenon have emerged as the prime choices to study the formation mechanism of various defects in continuous casting slabs. However, in various forms, the conventional hydrodynamic problems, such as the high-temperature melt multiphase flow in various metallurgical reactors, is characterized by a considerable change in physical properties, complex constitutive equations, diverse influencing factors of phase interface, and large gradient of physical quantities near the boundary. In addition, in the multiphysical fields inside continuous casting mold, there exists complex and variable multiscale interface phenomena like large-scale interface deformation of the continuous phase, transport of discrete phase particle, and transition between continuous and discrete phase, as well as the multiscale turbulent vortex structure, which poses a great challenge to modeling of high-temperature melt multiphase flow. Compared with the single-phase flow, the multiphase flow is characterized by the topological variation of the phase interface. In this paper, the research progress on modeling the high-temperature melt multiphase flow in the continuous casting mold is discussed from the following four perspectives: the scale distribution of discrete flow interface, cross-scale phenomenon of mixed flow interface, multiscale phenomenon of solidification interface, and role of turbulence in revealing the multiscale phase interface structure. Finally, the potential study direction in the future is considered.

Key words: continuous casting mold    high-temperature melt    multiphase flow    multiscale    modeling
收稿日期: 2022-04-17     
ZTFLH:  TF777.1  
基金资助:国家自然科学基金项目(51974071);国家自然科学基金项目(52171031);中国博士后科学基金项目(2020M680475)
作者简介: 刘中秋,男,1986年生,副教授,博士
图1  结晶器内多相、多物理场、多尺度特征
图2  不同粒径气泡的运动轨迹[25]
图3  实际连铸坯内气泡及夹杂物空间分布[12]
图4  结晶器内的气泡群与脱群气泡
图5  夹杂物在凝固坯壳上的捕捉位置[10]
图6  结晶器上表面的渣眼分布[51]
图7  实验与模拟水口内含气率分布对比
图8  水模型实验中的漩涡卷渣现象[78]
图9  水模型实验中的乳化现象[51]
图10  数值模拟捕捉到的漩涡卷渣现象[52]
图11  底部视角下的气泡聚并过程[109]
图12  凝固实验捕捉到的宏观凝固组织演化[128,129]
图13  钢带初始温度(Td0)与等轴晶率的关系[129]
MethodContinuityMomentum equationSolvable scaleModelComputation
equationrequirement
DNS∂ui∂xi=0∂ui∂t+uj∂ui∂xj=Eddies of all scalesNoHuge
-1ρ∂p∂xj+υ∂2ui∂xj∂xj+fi
LES∂u¯i∂xi=0∂u¯i∂t+uj∂uiuj¯∂xj=Eddies of large scalesSubgrid scale modelHigh
-1ρ∂p¯∂xj+υ∂2u¯i∂xj∂xj+f¯i
RANS∂ui∂xi=0∂ui∂t+∂uiuj∂xj=Eddies of average scaleTime-averaged turbulence modelLow
-1ρ∂p∂xj+υ∂2ui∂xj∂xj+fi
表1  3种湍流数值模拟方法的基本方程和特点
图14  结晶器内钢液-Ar气两相瞬态流场特征[50]
1 Li B K, Liu Z Q. Computational Fluid Dynamics in Steelmaking Processes [M]. Beijing: Metallurgical Industry Press, 2016: 1
1 李宝宽, 刘中秋. 炼钢中的计算流体力学 [M]. 北京: 冶金工业出版社, 2016: 1
2 Li B K, Okane T, Umeda T. Modeling of molten metal flow in a continuous casting process considering the effects of argon gas injection and static magnetic-field application [J]. Metall. Mater. Trans., 2000, 31B: 1491
3 Li B K, Okane T, Umeda T. Modeling of biased flow phenomena associated with the effects of static magnetic-field application and argon gas injection in slab continuous casting of steel [J]. Metall. Mater. Trans., 2001, 32B: 1053
4 Li B K, Tsukihashi F. Numerical estimation of the effect of the magnetic field application on the motion of inclusion in continuous casting of steel [J]. ISIJ Int., 2003, 43: 923
doi: 10.2355/isijinternational.43.923
5 Li B K, Huo H F, Luan Y J. Effects of magnetic field and argon gas injection on the inclusion motion in flow control mold [J]. Acta Metall. Sin., 2003, 39: 932
5 李宝宽, 霍慧芳, 栾叶君. 流动控制结晶器内磁场和吹氩对夹杂物粒子群运动的影响 [J]. 金属学报, 2003, 39: 932
6 Li W B, Wang F, Qi F S, et al. Mathematical model on steel strip-feeding of mold in continuous casting process [J]. Acta Metall. Sin., 2007, 43: 1191
6 李维彪, 王 芳, 齐凤升 等. 结晶器喂钢带连铸坯凝固过程的数学模拟 [J]. 金属学报, 2007, 43: 1191
7 Li B K, Dai F Y, Qi F S, et al. Flow field and concentration field of alloying addition in clad steel continuous casting mold using long and short nozzles [J]. Acta Metall. Sin., 2010, 46: 736
doi: 10.3724/SP.J.1037.2010.00736
7 李宝宽, 代凤羽, 齐凤升 等. 双水口注流连铸复合钢坯结晶器流场和合金元素浓度场研究 [J]. 金属学报, 2010, 46: 736
doi: 10.3724/SP.J.1037.2010.00025
8 Gan Y, Tang H W, Qiu S T. Function of continuous cast steel in steel production process and brief introduction of modern continuous casting technology [J]. Sci. China, 2008, 38E: 1384
8 干 勇, 唐红伟, 仇圣桃. 连续铸钢在钢铁生产流程中的作用及现代连铸技术简介 [J]. 中国科学, 2008, 38E: 1384
9 Liu Z Q, Li B K, Zhang L, et al. Analysis of transient transport and entrapment of particle in continuous casting mold [J]. ISIJ Int., 2014, 54: 2324
doi: 10.2355/isijinternational.54.2324
10 Liu Z Q, Li B K. Transient motion of inclusion cluster in vertical-bending continuous casting caster considering heat transfer and solidification [J]. Powder Technol., 2016, 287: 315
doi: 10.1016/j.powtec.2015.10.025
11 Liu Z Q, Li B K. Effect of vertical length on asymmetric flow and inclusion transport in vertical-bending continuous caster [J]. Powder Technol., 2018, 323: 403
doi: 10.1016/j.powtec.2017.10.034
12 Liu Z Q, Li B K, Wu M H, et al. An experimental benchmark of non-metallic inclusion distribution inside a heavy continuous-casting slab [J]. Metall. Mater. Trans., 2019, 50A: 1370
13 Miki Y, Takeuchi S. Internal defects of continuous casting slabs caused by asymmetric unbalanced steel flow in mold [J]. ISIJ Int., 2003, 43: 1548
doi: 10.2355/isijinternational.43.1548
14 Zhang L F, Thomas B G. State of the art in evaluation and control of steel cleanliness [J]. ISIJ Int., 2003, 43: 271
doi: 10.2355/isijinternational.43.271
15 Zhou Y H, Hu Z Q, Jie W Q. Solidification Technology [M]. Beijing: China Machine Press, 1998: 1
15 周尧和, 胡壮麒, 介万奇. 凝固技术 [M]. 北京: 机械工业出版社, 1998: 1
16 Li J, Xia M X, Hu Q D, et al. Solutions in improving homogeneities of heavy ingots [J]. Acta Metall. Sin., 2018, 54: 773
doi: 10.11900/0412.1961.2017.00525
16 李 军, 夏明许, 胡侨丹 等. 大型铸锭均质化问题及其新解 [J]. 金属学报, 2018, 54: 773
17 Zhang W W, Ke P, Yang C X, et al. Progress of computability of multi-scale interface problems in gas-liquid two-phase flow [J]. CIESC J, 2014, 65: 4645
17 张文伟, 柯 鹏, 杨春信 等. 气液两相流界面多尺度问题可计算性研究进展 [J]. 化工学报, 2014, 65: 4645
18 Zheng S G, Zhu M Y. Study on mechanism of large bubble formation in slab continuous casting mould with argon blowing [J]. Steel Res. Int., 2008, 79: 918
doi: 10.1002/srin.200806221
19 Wu S Z, Li Z Z. Research of gas-containing ratio and argon bubbles distribution law in ultra-wide slab continuous casting mold [J]. Metal. Int., 2011, 16: 5
20 Srinivas P S, Singh A, Korath J M, et al. Multiphase vortex flow patterns in slab caster mold: Experimental study [J]. ISIJ Int., 2017, 57: 1553
doi: 10.2355/isijinternational.ISIJINT-2017-062
21 Srinivas P S, Korath J M, Jana A K. Multiphase vortex flow patterns in slab caster mould: Insights of air vortex interaction and plant data analysis [J]. Can. Metall. Q., 2020, 59: 270
doi: 10.1080/00084433.2020.1732689
22 Ramos-Banderas A, Morales R D, Sánchez-Pérez R, et al. Dynamics of two-phase downwards flows in submerged entry nozzles and its influence on the two-phase flow in the mold [J]. Int. J. Multiphase Flow, 2005, 31: 643
doi: 10.1016/j.ijmultiphaseflow.2005.01.010
23 Lee G G, Thomas B G, Kim S H. Effect of refractory properties on initial bubble formation in continuous-casting nozzles [J]. Met. Mater. Int., 2010, 16: 501
doi: 10.1007/s12540-010-0601-y
24 Cho S M, Thomas B G, Kim S H. Bubble behavior and size distributions in stopper-rod nozzle and mold during continuous casting of steel slabs [J]. ISIJ Int., 2018, 58: 1443
doi: 10.2355/isijinternational.ISIJINT-2018-096
25 Wu Y D, Liu Z Q, Wang F, et al. Experimental investigation of trajectories, velocities and size distributions of bubbles in a continuous-casting mold [J]. Powder Technol., 2021, 387: 325
doi: 10.1016/j.powtec.2021.04.015
26 Chen Z H, Wang E G, Zhang X W, et al. Study on the behaviour of bubbles in a continuous casting mold with Ar injection and traveling magnetic field [J]. Acta Metall. Sin., 2012, 48: 951
doi: 10.3724/SP.J.1037.2011.00792
26 陈芝会, 王恩刚, 张兴武 等. 行波磁场下吹Ar过程中结晶器内气泡行为的研究 [J]. 金属学报, 2012, 48: 951
doi: 10.3724/SP.J.1037.2011.00792
27 Timmel K, Eckert S, Gerbeth G, et al. Experimental modeling of the continuous casting process of steel using low melting point metal alloys—The LIMMCAST program [J]. ISIJ Int., 2010, 50: 1134
doi: 10.2355/isijinternational.50.1134
28 Timmel K, Shevchenko N, Röder M, et al. Visualization of liquid metal two-phase flows in a physical model of the continuous casting process of steel [J]. Metall. Mater. Trans., 2015, 46B: 700
29 Ren Z M, Zhang Z Q, Deng K, et al. Experimental investigation of fluid flow in CC mold with electromagnetic filed [J]. J. Iron Steel Res. Int., 2011, 18(S2): 227
30 Zhang H H, Wang W L, Zhou D, et al. A study for initial solidification of Sn-Pb alloy during continuous casting: Part I. The development of the technique [J]. Metall. Mater. Trans., 2014, 45B: 1038
31 Zhou D, Wang W L, Zhang H H, et al. A study for initial solidification of Sn-Pb alloy during continuous casting: Part II. Effects of casting parameters on initial solidification and shell surface [J]. Metall. Mater. Trans., 2014, 45B: 1048
32 Miyake T, Morishita M, Nakata H, et al. Influence of sulphur content and molten steel flow on entrapment of bubbles to solid/liquid interface [J]. ISIJ Int., 2006, 46: 1817
doi: 10.2355/isijinternational.46.1817
33 Damen W, Abbel G. Argon bubbles in slabs, a non-homogeneous distribution [J]. Rev. Metall., 1997, 94: 745
doi: 10.1051/metal/199794060745
34 Naveau P, Visser H H, Galpin J M, et al. An investigation on the mechanism of gas bubbles/inclusions entrapment in the solidified steel shell [A]. 5th European Continuous Casting Conference [C]. Nice, France, June 20-22, 2005
35 Thomas B G, Yuan Q, Mahmood S, et al. Transport and entrapment of particles in steel continuous casting [J]. Metall. Mater. Trans., 2014, 45B: 22
36 Cho S M, Thomas B G, Kim S H. Transient two-phase flow in slide-gate nozzle and mold of continuous steel slab casting with and without double-ruler electro-magnetic braking [J]. Metall. Mater. Trans., 2016, 47B: 3080
37 Pfeiler C, Thomas B G, Wu M, et al. Solidification and particle entrapment during continuous casting of steel [J]. Steel Res. Int., 2008, 79: 599
doi: 10.1002/srin.200806172
38 Chen W, Zhang L F. Effects of interphase forces on multiphase flow and bubble distribution in continuous casting strands [J]. Metall. Mater. Trans., 2021, 52B: 528
39 Zhang L F, Wang Y F. Modeling the entrapment of nonmetallic inclusions in steel continuous-casting billets [J]. JOM, 2012, 64: 1063
doi: 10.1007/s11837-012-0421-2
40 Liu Z Q, Li B K, Jiang M F. Transient asymmetric flow and bubble transport inside a slab continuous-casting mold [J]. Metall. Mater. Trans., 2014, 45B: 675
41 Liu Z Q, Li Z M, Li B K, et al. Large eddy simulation of transient flow, solidification, and particle transport processes in continuous-casting mold [J]. JOM, 2014, 66: 1184
doi: 10.1007/s11837-014-1010-3
42 Liu C L, Luo Z G, Zhang T, et al. Mathematical modeling of multi-sized argon gas bubbles motion and its impact on melt flow in continuous casting mold of steel [J]. J. Iron Steel Res. Int., 2014, 21: 403
doi: 10.1016/S1006-706X(14)60062-5
43 Yin Y B, Zhang J M, Ma H T, et al. Large eddy simulation of transient flow, particle transport, and entrapment in slab mold with double-ruler electromagnetic braking [J]. Steel Res. Int., 2021, 92: 2000582
doi: 10.1002/srin.202000582
44 Zhang T, Luo Z G, Zhou H, et al. Analysis of two-phase flow and bubbles behavior in a continuous casting mold using a mathematical model considering the interaction of bubbles [J]. ISIJ Int., 2016, 56: 116
doi: 10.2355/isijinternational.ISIJINT-2015-456
45 Yang H, Vanka S P, Thomas B G. A hybrid Eulerian-Eulerian discrete-phase model of turbulent bubbly flow [J]. J. Fluids Eng., 2018, 140: 101202
doi: 10.1115/1.4039793
46 Sarkar S, Singh V, Ajmani S K, et al. Effect of argon injection in meniscus flow and turbulence intensity distribution in continuous slab casting mold under the influence of double ruler magnetic field [J]. ISIJ Int., 2018, 58: 68
doi: 10.2355/isijinternational.ISIJINT-2017-448
47 Bai H, Thomas B G. Turbulent flow of liquid steel and argon bubbles in slide-gate tundish nozzles: Part I. Model development and validation [J]. Metall. Mater. Trans., 2001, 32B: 253
48 Bai H, Thomas B G. Turbulent flow of liquid steel and argon bubbles in slide-gate tundish nozzles: Part II. Effect of operation conditions and nozzle design [J]. Metall. Mater. Trans., 2001, 32B: 269
49 Kubo N, Ishii T, Kubota J, et al. Two-phase flow numerical simulation of molten steel and argon gas in a continuous casting mold [J]. ISIJ Int., 2002, 42: 1251
doi: 10.2355/isijinternational.42.1251
50 Liu Z Q, Li B K. Large-eddy simulation of transient horizontal gas-liquid flow in continuous casting using dynamic subgrid-scale model [J]. Metall. Mater. Trans., 2017, 48B: 1833
51 Liu Z Q, Li B K, Vakhrushev A, et al. Physical and numerical modeling of exposed slag eye in continuous casting mold using Euler-Euler approach [J]. Steel Res. Int., 2019, 90: 1800117
doi: 10.1002/srin.201800117
52 Liu Z Q, Sun Z B, Li B K. Modeling of quasi-four-phase flow in continuous casting mold using hybrid Eulerian and Lagrangian approach [J]. Metall. Mater. Trans., 2017, 48B: 1248
53 Liu Z Q, Li B K, Jiang M F, et al. Euler-Euler-Lagrangian modeling for two-phase flow and particle transport in continuous casting mold [J]. ISIJ Int., 2014, 54: 1314
doi: 10.2355/isijinternational.54.1314
54 Liu Z Q, Li L M, Qi F S, et al. Population balance modeling of polydispersed bubbly flow in continuous-casting using multiple-size-group approach [J]. Metall. Mater. Trans., 2015, 46B: 406
55 Liu Z Q, Qi F S, Li B K, et al. Multiple size group modeling of polydispersed bubbly flow in the mold: An analysis of turbulence and interfacial force models [J]. Metall. Mater. Trans., 2015, 46B: 933
56 Li L M, Liu Z Q, Li B K. Modelling of bubble aggregation, breakage and transport in slab continuous casting mold [J]. J. Iron Steel Res. Int., 2015, 22: 30
57 Liu Z Q, Qi F S, Li B K, et al. Modeling of bubble behaviors and size distribution in a slab continuous casting mold [J]. Int. J. Multiphase Flow, 2016, 79: 190
doi: 10.1016/j.ijmultiphaseflow.2015.07.009
58 Wu Y D, Liu Z Q, Li B K, et al. Numerical simulation of multi-size bubbly flow in a continuous casting mold using population balance model [J]. Powder Technol., 2022, 396: 224
doi: 10.1016/j.powtec.2021.10.055
59 Liu Z Q, Li B K, Qi F S, et al. Population balance modeling of polydispersed bubbly flow in continuous casting using average bubble number density approach [J]. Powder Technol., 2017, 319: 139
doi: 10.1016/j.powtec.2017.06.034
60 Prince M J, Blanch H W. Bubble coalescence and break-up in air-sparged bubble columns [J]. AIChE J., 1990, 36: 1485
doi: 10.1002/aic.690361004
61 Luo H A, Svendsen H F. Theoretical model for drop and bubble breakup in turbulent dispersions [J]. AIChE J., 1996, 42: 1225
doi: 10.1002/aic.690420505
62 Wu Q, Kim S, Ishii M, et al. One-group interfacial area transport in vertical bubbly flow [J]. Int. J. Heat Mass Transfer, 1998, 41: 1103
doi: 10.1016/S0017-9310(97)00167-1
63 Hibiki T, Ishii M. Two-group interfacial area transport equations at bubbly-to-slug flow transition [J]. Nucl. Eng. Des., 2000, 202: 39
doi: 10.1016/S0029-5493(00)00286-7
64 Teshima T, Kubota J, Suzuki M, et al. Influence of casting conditions on molten steel flow in continuous casting mold at high speed casting of slabs [J]. Tetsu Hagané, 1993, 79(5): 40
64 手嶋 俊雄, 久保田 淳, 鈴木 幹雄 等. スラブ高速鋳造時の連鋳鋳型内溶鋼流動におよぼす鋳造条件の影響 [J]. 鉄と鋼, 1993, 79(5): 40
65 Gupta D, Lahiri A K. Cold model study of the surface profile in a continuous slab casting mold: Effect of second phase [J]. Metall. Mater. Trans., 1994, 27B: 695
66 Kumar D S, Rajendra T, Sarkar A, et al. Slab quality improvement by controlling mould fluid flow [J]. Ironmaking Steelmaking, 2007, 34: 185
doi: 10.1179/174328107X155330
67 Zhang L F, Yang S B, Cai K K, et al. Investigation of fluid flow and steel cleanliness in the continuous casting strand [J]. Metall. Mater. Trans., 2007, 38B: 63
68 Iguchi M, Yoshida J, Shimizu T, et al. Model study on the entrapment of mold powder into molten steel [J]. ISIJ Int., 2000, 40: 685
doi: 10.2355/isijinternational.40.685
69 Li B K, Li D H. Water model observation and numerical simu-lation of vortexing flow at molten steel surface in continuous casting mold [J]. Acta Metall. Sin., 2002, 38: 315
69 李宝宽, 李东辉. 连铸结晶器内钢液涡流现象的水模型观察和数值模拟 [J]. 金属学报, 2002, 38: 315
70 Mills K C, Fox A B. The role of mould fluxes in continuous casting—So simple yet so complex [J]. ISIJ Int., 2003, 43: 1479
doi: 10.2355/isijinternational.43.1479
71 Zhang S J, Zhu M Y, Zhang Y L, et al. Study on mechanism of entrapment in slab continuous casting mould with high casting speed and argon blowing [J]. Acta Metall. Sin., 2006, 42: 1087
71 张胜军, 朱苗勇, 张永亮 等. 高拉速吹氩板坯连铸结晶器内的卷渣机理研究 [J]. 金属学报, 2006, 42: 1087
72 Hibbeler L C, Thomas B G. Mold slag entrainment mechanisms in continuous casting molds [J]. Iron Steel Technol., 2013, 10: 121
73 Hagemann R, Schwarze R, Heller H P, et al. Model investigations on the stability of the steel-slag interface in continuous-casting process [J]. Metall. Mater. Trans., 2013, 44B: 80
74 Zhang L, Li Y, Wang Q, et al. Prediction model for steel/slag interfacial instability in continuous casting process [J]. Ironmaking Steelmaking, 2015, 42: 705
doi: 10.1179/1743281215Y.0000000023
75 Asai S. Fluid flow and mass transfer in a refining process by use of stirring [A]. Proceedings of the 100 and 101 Nishiyama Memorial Lecture [C]. Tokyo: The Iron and Steel Institute of Japan, 1984: 65
76 Harman J M, Cramb A W. A study of the effect of fluid physical properties upon droplet emulsification [A]. 79th Steelmaking Conference [C]. Pittsburgh, PA: The Iron and Steel Society, 1996, 55: 773
77 Tozawa H, Idogawa A, Nakato H, et al. Investigation of periodical change of molten steel flow and entrainment of mold powder in continuous casting mold [J]. CAMP-ISIJ, 1996, 9: 604
77 戸沢宏一, 井戸川聡, 中戸参 等. 連鋳鋳型内における溶鋼流動の周期的変動とパウダ巻き込み挙動の解析 [J]. 材料とプロセス (日本鉄鋼協会講演論文集), 1996, 9: 604
78 Liu Z Q, Qi F S, Li B K, et al. Vortex flow pattern in a slab continuous casting mold with argon gas injection [J]. J. Iron Steel Res. Int., 2014, 21: 1081
doi: 10.1016/S1006-706X(14)60187-4
79 Bai H, Thomas B G. Effects of clogging, argon injection, and continuous casting conditions on flow and air aspiration in submerged entry nozzles [J]. Metall. Mater. Trans., 2001, 32B: 707
80 Li B K, Tsukihashi F. Vortexing flow patterns in a water model of slab continuous casting mold [J]. ISIJ Int., 2005, 45: 30
doi: 10.2355/isijinternational.45.30
81 Li B K, Tsukihashi F. Effects of electromagnetic brake on vortex flows in thin slab continuous casting mold [J]. ISIJ Int., 2006, 46: 1833
doi: 10.2355/isijinternational.46.1833
82 Mahmood S. Efficient modeling of flow asymmetries and particle entrapment in nozzle and mold during continuous casting of steel slabs [D]. Urbana: University of Illinois at Urbana-Champaign, 2006
83 Zhang L F, Wang Y F, Zuo X J. Flow transport and inclusion motion in steel continuous-casting mold under submerged entry nozzle clogging condition [J]. Metall. Mater. Trans., 2008, 39B: 534
84 Lee G G, Shin H J, Thomas B G, et al. Asymmetric multi-phase fluid flow and particle entrapment in a continuous casting mold [A]. AISTech 2008 [C]. Pittsburgh: AISTech, 2008: 63
85 Cho S M, Lee G G, Kim S H, et al. Effect of stopper-rod misalignment on asymmetric flow and vortex formation in steel slab casting [A]. Proceedings of Jim Evans Honorary Symposium-Held During TMS 2010 Annual Meeting and Exhibition [C]. Washington, February 14- 18, 2010: 71
86 Chaudhary R, Lee G G, Thomas B G, et al. Effect of stopper-rod misalignment on fluid flow in continuous casting of steel [J]. Metall. Mater. Trans., 2011, 42B: 300
87 Yamashita S, Iguchi M. Mechanism of mold powder entrapment caused by large argon bubble in continuous casting mold [J]. ISIJ Int., 2001, 41: 1529
doi: 10.2355/isijinternational.41.1529
88 Iguchi M, Sumida Y, Okada R, et al. Evaluation of critical gas flow rate for the entrapment of slag using a water model [J]. ISIJ Int., 1994, 34: 164
doi: 10.2355/isijinternational.34.164
89 Chung Y, Cramb A W. Dynamic and equilibrium interfacial phenomena in liquid steel-slag systems [J]. Metall. Mater. Trans., 2000, 31B: 957
90 Han Z J, Holappa L. Bubble bursting phenomenon in gas/metal/slag systems [J]. Metall. Mater. Trans., 2003, 34B: 525
91 Emling W H, Waugaman T A, Feldbauer S L, et al. Subsurface mold slag entrainment in ultra low carbon steels [A]. 77th Steelmaking Conference [C]. Chicago, IL: The Iron and Steel Society, 1994, 77: 371
92 Wang Z, Mukai K, Ma Z Y, et al. Influence of injected Ar gas on the involvement of the mold powder under different wettabilities between porous refractory and molten steel [J]. ISIJ Int., 1999, 39: 795
doi: 10.2355/isijinternational.39.795
93 Hahn I, Neuschütz D. Ejection of steel and slag droplets from gas stirred steel melts [J]. Ironmaking Steelmaking, 2002, 29: 219
doi: 10.1179/030192302225004115
94 Yoshida J, Iguchi M, Yokoya S. Water model experiment on mold powder entrapment around the exit of immersion nozzle in continuous casting mold [J]. Tetsu Hagané, 2001, 87: 9
94 吉田 仁, 井口 学, 横谷 真一郎. 連続鋳造モールド内浸漬ノズル吐出口近傍におけるモールドパウダー巻き込みに関する水モデル実験 [J]. 鉄と鋼, 2001, 87: 9
95 Yuan Z F, Huang W L, Mukai K. Local corrosion of magnesia-chrome refractories driven by Marangoni convection at the slag-metal interface [J]. J. Colloid Interface Sci., 2002, 253: 211
doi: 10.1006/jcis.2002.8504
96 Zhou L J, Wang W L, Liu R, et al. Computational modeling of temperature, flow, and crystallization of mold slag during double hot thermocouple technique experiments [J]. Metall. Mater. Trans., 2013, 44B: 1264
97 Real-Ramirez C A, Gonzalez-Trejo J I. Analysis of three-dimensional vortexes below the free surface in a continuous casting mold [J]. Int. J. Miner. Metall. Mater., 2011, 18: 397
doi: 10.1007/s12613-011-0453-6
98 Lopez P E R, Jalali P N, Björkvall J, et al. Recent developments of a numerical model for continuous casting of steel: Model theory, setup and comparison to physical modelling with liquid metal [J]. ISIJ Int., 2014, 54: 342
doi: 10.2355/isijinternational.54.342
99 Zhao P, Li Q, Kuang S B, et al. Mathematical modeling of liquid slag layer fluctuation and slag droplets entrainment in a continuous casting mold based on VOF-LES method [J]. High Temp. Mater. Processes, 2017, 36: 551
doi: 10.1515/htmp-2016-0143
100 Li X L, Li B K, Liu Z Q, et al. Large eddy simulation of electromagnetic three-phase flow in a round bloom considering solidified shell [J]. Steel Res. Int., 2019, 90: 1800133
doi: 10.1002/srin.201800133
101 Wang Y, Yang S F, Wang F, et al. Optimization on reducing slag entrapment in 150 × 1270 mm slab continuous casting mold [J]. Materials, 2019, 12: 1774
doi: 10.3390/ma12111774
102 Deng A Y, Xu L, Wang E G, et al. Numerical analysis of fluctuation behavior of steel/slag interface in continuous casting mold with static magnetic field [J]. J. Iron Steel Res. Int., 2014, 21: 809
doi: 10.1016/S1006-706X(14)60146-1
103 Jowsa J, Bielnicki M, Cwudziński A. Numerical modelling of metal/flux interface in a continuous casting mould [J]. Arch. Metall. Mater., 2015, 60: 2905
doi: 10.1515/amm-2015-0464
104 Zhao P, Zhou L H. Mathematical modelling of slag entrainment and entrained droplets in a continuous casting mould [J]. Ironmaking Steelmaking, 2019, 46: 886
doi: 10.1080/03019233.2019.1604613
105 Chen W, Zhang L F, Ren Q, et al. Large eddy simulation on four-phase flow and slag entrainment in the slab continuous casting mold [J]. Metall. Mater. Trans., 2022, 53B: 1446
106 Li L M, Li B K, Liu Z Q. Modeling of gas-steel-slag three-phase flow in ladle metallurgy: Part II. Multi-scale mathematical model [J]. ISIJ Int., 2017, 57: 1980
doi: 10.2355/isijinternational.ISIJINT-2017-069
107 Li X L, Li B K, Liu Z Q, et al. Large eddy simulation of multi-phase flow and slag entrapment in a continuous casting mold [J]. Metals, 2019, 9: 7
doi: 10.3390/met9010007
108 Li X L, Li B K, Liu Z Q, et al. Evaluation of slag entrapment in continuous casting mold based on the LES-VOF-DPM coupled model [J]. Metall. Mater. Trans., 2021, 52B: 3246
109 Sun M J, Li B K, Liu Z Q, et al. Experimental and numerical investigations on transient multiscale bubble behaviors in CuSO4 aqueous solution electrolysis cell [J]. Chem. Eng. J., 2022, 428: 131182
doi: 10.1016/j.cej.2021.131182
110 Tsukamoto K, Abe T, Sunagawa I. In situ observation of crystals growing in high temperature melts or solutions [J]. J. Cryst. Growth, 1983, 63: 215
doi: 10.1016/0022-0248(83)90452-9
111 Jie W Q, Zhou Y H. Modeling study of convection and constitution variation in ingot during solidification [J]. Acta Metall. Sin., 1988, 24: 457
111 介万奇, 周尧和. 铸锭凝固过程中的对流及液相区成分变化的模拟实验研究 [J]. 金属学报, 1988, 24: 457
112 Beckermann C, Viskanta R. Double-diffusive convection during dendritic solidification of a binary mixture [J]. PhysicoChem. Hydrodyn., 1988, 10: 195
113 Chen C F, Chen F L. Experimental study of directional solidification of aqueous ammonium chloride solution [J]. J. Fluid Mech., 1991, 227: 567
doi: 10.1017/S0022112091000253
114 Cao W Z, Poulikakos D. Transient solidification of a binary mixture in an inclined rectangular cavity [J]. J. Thermophys. Heat Transf., 1992, 6: 326
doi: 10.2514/3.363
115 Neilson D G, Incropera F P. Experimental study of unidirectional solidification of aqueous ammonium chloride in a cylindrical mold with and without rotation [J]. Exp. Heat Transfer, 1993, 6: 131
doi: 10.1080/08916159308946450
116 McCay M H, McCay T D, Hopkins J A. The nature and influence of convection on the directional dendritic solidification of a metal alloy analog, NH4Cl, and H2O [J]. Metall. Mater. Trans., 1993, 24B: 669
117 Beckermann C, Wang C Y. Equiaxed dendritic solidification with convection: Part III. Comparisons with NH4Cl-H2O experiments [J]. Metall. Mater. Trans., 1996, 27A: 2784
118 Wang S Y, Lin C X, Ebadian M A. Vortex flow of low concentration NH4Cl-H2O solution during the solidification process [J]. Int. J. Heat Mass Transfer, 1999, 42: 4153
doi: 10.1016/S0017-9310(99)00068-X
119 Wang S Y, Lin C X, Ebadian M A. Study of double-diffusive velocity during the solidification process using particle image velocimetry [J]. Int. J. Heat Mass Transfer, 1999, 42: 4427
doi: 10.1016/S0017-9310(99)00114-3
120 Duggirala R K, Lin C X, Ghenai C. Investigation of double-diffusive convection during the solidification of a binary mixture (NH4Cl-H2O) in a trapezoidal cavity [J]. Exp. Fluids, 2006, 40: 918
doi: 10.1007/s00348-006-0128-7
121 Huang W D, Zhang Y, Wang M, et al. In-situ observation of nucleation on a rough chilling surface in NH4Cl-H2O solution [J]. Trans. Indian Inst. Met., 2009, 62: 489
doi: 10.1007/s12666-009-0086-x
122 Kharicha A, Stefan-Kharicha M, Ludwig A, et al. Simultaneous observation of melt flow and motion of equiaxed crystals during solidification using a dual phase particle image velocimetry technique. Part II: Relative velocities [J]. Metall. Mater. Trans., 2013, 44A: 661
123 Zhou P, Wang M, Lin X, et al. Settling velocity of equiaxed dendrites in a tube [J]. Chin. Phys., 2013, 22B: 018101
124 Kharicha M S, Eck S, Könözsy L, et al. Experimental and numerical investigations of NH4Cl solidification in a mould Part 1: Experimental results [J]. Int. J. Cast Met. Res., 2009, 22: 168
doi: 10.1179/136404609X368000
125 Könözsy L, Eck S, Kharicha M S, et al. Experimental and numerical investigations of NH4Cl solidification in a mould Part 2: Numerical results [J]. Int. J. Cast Met. Res., 2013, 22: 172
doi: 10.1179/136404609X367605
126 Tian L, Bao Y P, Yang J T, et al. Characteristics of flow field during continuous casting solidifying process [J]. Iron Steel, 2013, 48(10): 36
126 田 陆, 包燕平, 杨建桃 等. 连铸凝固过程中的流动特征 [J]. 钢铁, 2013, 48(10): 36
127 Li X, Fautrelle Y, Ren Z M. Influence of thermoelectric effects on the solid-liquid interface shape and cellular morphology in the mushy zone during the directional solidification of Al-Cu alloys under a magnetic field [J]. Acta Mater., 2007, 55: 3803
doi: 10.1016/j.actamat.2007.02.031
128 Niu R, Li B K, Liu Z Q, et al. Experimental investigation of solidification in the cast mold with a consumable cooler introduced inside [J]. Metals, 2019, 9: 55
doi: 10.3390/met9010055
129 Liu Z Q, Niu R, Wu Y D, et al. Physical and numerical simulation of mixed columnar-equiaxed solidification during cold strip feeding in continuous casting [J]. Int. J. Heat Mass Transfer, 2021, 173: 121237
doi: 10.1016/j.ijheatmasstransfer.2021.121237
130 Flemings M C, Nereo G E. Macrosegregation: Part I [J]. Trans. Metall. Soc. AIME, 1967, 239: 1449
131 Bennon W D, Incropera F P. A continuum model for momentum, heat and species transport in binary solid-liquid phase change systems—I. Model formulation [J]. Int. J. Heat Mass Transfer, 1987, 30: 2161
doi: 10.1016/0017-9310(87)90094-9
132 Li L M, Liu Z Q, Li B K. Fluid flow and solute transport in the solidifying process of large steel ingots with top heating [A]. Proceedings of International Symposium on Liquid Metal Processing and Casting [C]. Leoben, Austria: The Minerals, Metals, and Materials Society, 2015
133 Ni J, Beckermann C. A volume-averaged two-phase model for transport phenomena during solidification [J]. Metall. Mater. Trans., 1991, 22B: 349
134 Li W S, Shen H F, Liu B C. Numerical simulation of macrosegregation in steel ingots using a two-phase model [J]. Int. J. Miner., Metall. Mater., 2012, 19: 787
135 Wu M H, Ludwig A. A three-phase model for mixed columnar-equiaxed solidification [J]. Metall. Mater. Trans., 2006, 37A: 1613
136 Wu M, Fjeld A, Ludwig A. Modelling mixed columnar-equiaxed solidification with melt convection and grain sedimentation-Part I: Model description [J]. Comput. Mater. Sci., 2010, 50: 32
doi: 10.1016/j.commatsci.2010.07.005
137 Zhu M F, Hong C P, Stefanescu D M, et al. Computational modeling of microstructure evolution in solidification of aluminum alloys [J]. Metall. Mater. Trans., 2007, 38B: 517
138 Yin H, Felicelli S D, Wang L. Simulation of a dendritic microstructure with the lattice Boltzmann and cellular automaton methods [J]. Acta Mater., 2011, 59: 3124
doi: 10.1016/j.actamat.2011.01.052
139 Chen R, Xu Q Y, Liu B C. A modified cellular automaton model for the quantitative prediction of equiaxed and columnar dendritic growth [J]. J. Mater. Sci. Technol., 2014, 30: 1311
doi: 10.1016/j.jmst.2014.06.006
140 Li B K, Wang Q, Wang F, et al. A coupled cellular automaton-finite-element mathematical model for the multiscale phenomena of electroslag remelting H13 die steel ingot [J]. JOM, 2014, 66: 1153
doi: 10.1007/s11837-014-0979-y
141 Wang Q, Yan H G, Wang F, et al. Impact of electromagnetic stirring on grain structure of electroslag remelting ingot [J]. JOM, 2015, 67: 1821
doi: 10.1007/s11837-015-1479-4
142 Niu R, Li B K, Liu Z Q, et al. Melting of moving strip during steel strip feeding in continuous casting process [J]. Steel Res. Int., 2018, 89: 1700407
doi: 10.1002/srin.201700407
143 Niu R, Li B K, Liu Z Q, et al. Effect of strip feeding into mold on fluid flow and heat transfer in continuous casting process [J]. J. Iron Steel Res. Int., 2020, 27: 295
doi: 10.1007/s42243-019-00341-8
144 Thomas B G, Mika L J, Najjar F M. Simulation of fluid flow inside a continuous slab-casting machine [J]. Metall. Mater. Trans., 1990, 21B: 387
145 Anagnostopoulos J, Bergeles G. Three-dimensional modeling of the flow and the interface surface in a continuous casting mold model [J]. Metall. Mater. Trans., 1999, 30B: 1095
146 Li B K, Tsukihashi F. Effect of static magnetic field application on the mass transfer in sequence slab continuous casting process [J]. ISIJ Int., 2001, 41: 844
doi: 10.2355/isijinternational.41.844
147 Kwon Y, Zhang J, Lee H G. Water model and CFD studies of bubble dispersion and inclusions removal in continuous casting mold of steel [J]. ISIJ Int., 2006, 46: 257
doi: 10.2355/isijinternational.46.257
148 Li B K, Gu M Y, Qi F S, et al. Modeling of three-phase (gas/molten steel/slag) flows and slag layer behavior in an argon gas stirred ladle [J]. Acta Metall. Sin., 2008, 44: 1198
148 李宝宽, 顾明言, 齐凤升 等. 底吹钢包内气/钢液/渣三相流模型及渣层行为的研究 [J]. 金属学报, 2008, 44: 1198
149 Chaudhary R, Ji C, Thomas B G, et al. Transient turbulent flow in a liquid-metal model of continuous casting, including comparison of six different methods [J]. Metall. Mater. Trans., 2011, 42B: 987
150 Zhang X W, Jin X L, Wang Y, et al. Comparison of standard k-ε model and RSM on three dimensional turbulent flow in the SEN of slab continuous caster controlled by slide gate [J]. ISIJ Int., 2011, 51: 581
doi: 10.2355/isijinternational.51.581
151 Ren B Z, Chen D F, Wang H D, et al. Numerical simulation of fluid flow and solidification in bloom continuous casting mould with electromagnetic stirring [J]. Ironmaking Steelmaking, 2015, 42: 401
doi: 10.1179/1743281214Y.0000000240
152 Liu Z Q, Li B K, Tsukihashi F. Instability and periodicity of asymmetrical flow in a funnel thin slab continuous casting mold [J]. ISIJ Int., 2015, 55: 805
doi: 10.2355/isijinternational.55.805
153 Li B K, Liu Z Q, Qi F S, et al. Large eddy simulation for unsteady turbulent flow in thin slab continuous casting mold [J]. Acta Metall. Sin., 2012, 48: 23
doi: 10.3724/SP.J.1037.2011.00464
153 李宝宽, 刘中秋, 齐凤升 等. 薄板坯连铸结晶器非稳态湍流大涡模拟研究 [J]. 金属学报, 2012, 48: 23
doi: 10.3724/SP.J.1037.2011.00464
154 Liu Z Q, Qi F S, Li B K, et al. Large eddy simulation for unsteady turbulent field in thin slab continuous casting mold [J]. J. Iron Steel Res. Int., 2011, 18: 243
155 Liu Z Q, Li L M, Li B K. Large eddy simulation of transient flow and inclusions transport in continuous casting mold under different electromagnetic brakes [J]. JOM, 2016, 68: 2180
doi: 10.1007/s11837-016-1988-9
156 Liu Z Q, Vakhrushev A, Wu M H, et al. Effect of an electrically-conducting wall on transient magnetohydrodynamic flow in a continuous-casting mold with an electromagnetic brake [J]. Metals, 2018, 8: 609
doi: 10.3390/met8080609
157 Zhu M Y, Lou W T, Wang W L. Research progress of numerical simulation in steelmaking and continuous casting processes [J]. Acta Metall. Sin., 2018, 54: 131
157 朱苗勇, 娄文涛, 王卫领. 炼钢与连铸过程数值模拟研究进展 [J]. 金属学报, 2018, 54: 131
158 Wang Q, He M, Zhu X W, et al. Study and development on numerical simulation for application of electromagnetic field technology in metallurgical processes [J]. Acta Metall. Sin., 2018, 54: 228
158 王 强, 何 明, 朱晓伟 等. 电磁场技术在冶金领域应用的数值模拟研究进展 [J]. 金属学报, 2018, 54: 228
159 Wang B, Shen S Y, Ruan Y W, et al. Simulation of gas-liquid two-phase flow in metallurgical process [J]. Acta Metall. Sin., 2020, 56: 619
159 王 波, 沈诗怡, 阮琰炜 等. 冶金过程中的气液两相流模拟 [J]. 金属学报, 2020, 56: 619
160 Liu Z Q, Li B K, Jiang M F, et al. Large eddy simulation of unsteady argon/steel two phase turbulent flow in a continuous casting mold [J]. Acta Metall. Sin., 2013, 49: 513
doi: 10.3724/SP.J.1037.2012.00760
160 刘中秋, 李宝宽, 姜茂发 等. 连铸结晶器内氩气/钢液两相非稳态湍流特性的大涡模拟研究 [J]. 金属学报, 2013, 49: 513
doi: 10.3724/SP.J.1037.2012.00760
161 Liu Z Q, Li B K, Jiang M F, et al. Modeling of transient two-phase flow in a continuous casting mold using Euler-Euler large eddy simulation scheme [J]. ISIJ Int., 2013, 53: 484
doi: 10.2355/isijinternational.53.484
162 Liu Z Q, Li B K. Scale-adaptive analysis of Euler-Euler large eddy simulation for laboratory scale dispersed bubbly flows [J]. Chem. Eng. J., 2018, 338: 465
doi: 10.1016/j.cej.2018.01.051
163 Liu Z Q, Vakhrushev A, Wu M H, et al. Scale-adaptive simulation of transient two-phase flow in continuous-casting mold [J]. Metall. Mater. Trans., 2019, 50B: 543
164 Liu Z Q, Wu Y D, Li B K, et al. An assessment on the performance of sub-grid scale models of large eddy simulation in modeling bubbly flows [J]. Powder Technol., 2020, 374: 470
doi: 10.1016/j.powtec.2020.07.055
[1] 李时磊, 李阳, 王友康, 王胜杰, 何伦华, 孙光爱, 肖体乔, 王沿东. 基于中子与同步辐射技术的工程材料/部件多尺度残余应力评价[J]. 金属学报, 2023, 59(8): 1001-1014.
[2] 王冠杰, 李开旗, 彭力宇, 张壹铭, 周健, 孙志梅. 高通量自动流程集成计算与数据管理智能平台及其在合金设计中的应用[J]. 金属学报, 2022, 58(1): 75-88.
[3] 兰亮云, 孔祥伟, 邱春林, 杜林秀. 基于多尺度力学实验的氢脆现象的最新研究进展[J]. 金属学报, 2021, 57(7): 845-859.
[4] 朱敏, 欧阳柳章. 镁基储氢合金动力学调控及电化学性能[J]. 金属学报, 2021, 57(11): 1416-1428.
[5] 刘兴军, 陈悦超, 卢勇, 韩佳甲, 许伟伟, 郭毅慧, 于金鑫, 魏振帮, 王翠萍. 新型钴基高温合金多尺度设计的研究现状与展望[J]. 金属学报, 2020, 56(1): 1-20.
[6] 周丽,张鹏飞,王全兆,肖伯律,马宗义,于涛. B4C/6061Al复合材料热压缩断裂行为的多尺度研究[J]. 金属学报, 2019, 55(7): 911-918.
[7] 李雄兵, 宋永锋, 倪培君, 刘锋. 面向晶粒尺寸的超声多尺度衰减评价方法[J]. 金属学报, 2015, 51(1): 121-128.
[8] 刘中秋,李宝宽,姜茂发,张立,徐国栋. 连铸结晶器内氩气/钢液两相非稳态湍流特性的大涡模拟研究[J]. 金属学报, 2013, 49(5): 513-522.
[9] 陈芝会 王恩刚 张兴武 王元华 朱明伟 赫冀成. 行波磁场下吹Ar过程中结晶器内气泡行为的研究[J]. 金属学报, 2012, 48(8): 951-956.
[10] 李宝宽 刘中秋 齐凤升 王芳 徐国栋. 薄板坯连铸结晶器非稳态湍流大涡模拟研究[J]. 金属学报, 2012, 48(1): 23-32.
[11] 刘相华. 塑性有限元在金属轧制过程中应用的进展[J]. 金属学报, 2010, 46(9): 1025-1033.
[12] 许秀杰 邓安元 王恩刚 张林涛 张兴武 张永杰 赫冀成. 电磁软接触连铸圆坯表面振痕演变机理[J]. 金属学报, 2009, 45(4): 464-469.
[13] 孟祥宁 朱苗勇. 高拉速板坯连铸结晶器液态渣消耗机理分析[J]. 金属学报, 2009, 45(4): 485-489.
[14] 黎军顽 倪玉山 林逸汉 罗诚 江五贵. Al薄膜纳米压痕过程的多尺度模拟[J]. 金属学报, 2009, 45(2): 129-136.
[15] 于海岐; 朱苗勇 . 板坯连铸结晶器电磁制动和吹氩过程的多相流动现象[J]. 金属学报, 2008, 44(5): 619-625 .