Due to their excellent performance, near α and α + β dual-phase titanium alloys are critical materials in aerospace engineering. Enhancing the performance stability of titanium alloy forgings has become a focal point of research in engineering applications. However, the microtextures within these forgings significantly affect key properties such as fatigue resistance, which limits the overall performance of titanium alloy forgings. Recent studies indicate that optimizing the hot working process to improve the crystallographic orientation and microstructure uniformity is an effective means of enhancing alloy performance. This study reviews the origins of microtextures in titanium alloy forgings, their potential negative effects, and the optimization processes involved. Finally, the study presents several research guidelines aimed at improving the microstructural uniformity of titanium alloy forgings.
Fig.1
Influences of hard-oriented primary α phase within macrozones on dwell-fatigue crack formation in titanium alloys[14] (a, c) SEM images showing the primary crack nucleation sites (b, d) crystallographic orientations relative to the loading direction in the same region (e) discrete pole figures (PFs) showing crystallographic orientations in locations numbered from 1 to 3 in Figs.1a and c (LD represents loading direction)
Fig.2
Influences of microtexture on tensile strength stability (a) and plasticity after thermal exposure (b) of Ti60 alloy (Rm and A denote the tensile strength and elongation at room temperature, respectively. CV represents coefficient of variation of strength. The multiple data in the figure are taken from forgings with strong and weak microtextures that have undergone the same heat treatment (Tβ - 20 oC, 2 h, AC + 700 oC, 6 h, AC, in which Tβ represents β transition temperature, AC represents air cooling)
Fig.3
Effects of primary α phase on variant selection during β→α transformation and its contribution to texture intensity in macrozone[33] (a, c) inverse pole figures (IPFs) of specimens after compression (960 oC, 0.1 s-1, 30%) and then heat treatments at 980 oC (a) and 990 oC (c) for 1 h (TD, RD, and CA denotes transverse direction, radial direction, and compression axial direction, respectively) (b, d) IPFs and PFs of microtextured areas from Figs.3a and c (αp—primary α, αs—secondary α)
Fig.4
Orientation distribution in different regions after spheroidization of lamellar α phase (The deformation conditions is 970 oC, 25%, 0.1 s-1. Ⅰ—twist zone, Ⅱ—β/β boundary, Ⅲ—α/α boundary, Ⅳ—non-twist zone)
Fig.5
In-grain misorientation axis analysis (IGMA) based on EBSD orientation measurement for α colonies with different orientations in Ti60 alloy[26,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points)
Fig.7
Microstructures and crystallographic orientation evolutions of Ti60 alloy with α lamellae structure during thermal deformation at 900 oC (a, c, e) and 980 oC (b, d, f) (a, b) SEM images (Insets show enlarged SEM images)[45] (CD—compression direction) (c, d) IPF orientation maps (Insets show PFs of α texture measured by the XRD method)[45] (e, f) TEM bright field images[26,45]
Fig.8
Schematics of the pinning effect of primary α phase on prior β grains during deformation (LAGB—low angle grain boundary, HAGB—high angle grain boundary)
(a) dislocation accumulation(b) formation of sub‑boundaries and grain boundaries(c) grain growth, rotation, and pinning by primary α phase
Fig.9
Evolutions of the αp/β phase boundary and its effects on microstructure during heat treatment of Ti60 alloy[26,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)
Fig.10
Microstructure and crystallographic orientation analyses of the TC17 bar after axial and radial compressions (a, b) IPF orientation maps of the deformed microstructure (a) and αp grains (b) (AD indicates axial direction of the bar)(c) BC map of αp grains with some special phase boundaries(d, e) interface structures of semi-coherent (d) and non-coherent (e) αp/β phase boundaries(f) θ distributions ( fθ ≥ 15° denotes the number fraction of θ ≥ 15°)
3D printing technology is a new type of precision forming technology and the core technology of the third industrial revolution. The powder-based 3D printing technology of titanium and its alloys have received great attention in biomedical applications since its advantages of custom manufacturing, cost-saving, time-saving, and resource-saving potential. In particular, the personalized customization of 3D printing can meet specific needs and achieve precise control of micro-organization and structural design. The purpose of this review is to present the most advanced multi-material 3D printing methods for titanium-based biomaterials. We first reviewed the bone tissue engineering, the application of titanium alloy as bone substitutes and the development of manufacturing technology, which emphasized the advantages of 3D printing technology over traditional manufacturing methods. What is more, the optimization design of the hierarchical structure was analyzed to achieve the best mechanical properties, and the biocompatibility and osseointegration ability of the porous titanium alloy after implantation in living bodies was analyzed. Finally, we emphasized the development of digital tools such as artificial intelligence, which provides new ideas for the rational selection of processing parameters. The 3D printing titanium-based alloys will meet the huge market demand in the biomedical field, but there are still many challenges, such as the trade-off between high strength and low modulus, optimization of process parameters and structural design. We believe that the combination of mechanical models, machine learning, and metallurgical knowledge may shape the future of metal printing.
YangY, ZhangB H, MengZ C, et al.
{332}<113> twinning transfer behavior and its effect on the twin shape in a beta-type Ti-23.1Nb-2.0Zr-1.0O alloy
The interaction between twins and grain boundaries (GB) has an important influence on the deformation and fracture behavior of materials. In the present work, {332}<113> twinning transfer (TT) behavior and its effect on the twin shape in a deformed β-type Ti-23.1Nb-2.0Zr-1.0O Ti alloy were investigated experimentally and with molecular dynamics simulation. The crystallographic alignment factor of the two twinning systems in the neighboring grains and the misorientation angle of the grain pairs were found to influence the occurrence of TT. This further determines the twin shape: twins present a ruler shape when TT occurs but are in a lenticular shape otherwise. Such different twin shapes are attributed to the local stress states related to TT occurring or not. Both ruler-shaped paired twinning and lenticular twinning would provide effective mechanisms to release or reduce the stress concentration in front of the twin tips in different grain pairs.
WangQ J, LiuJ R, YangR.
High temperature titanium alloys: Status and perspective
A heterogeneous microstructure in terms of local orientation distribution is often found in near-α titanium alloys. The presence of large regions with similar crystallographic orientation, called ‘macrozones’, could drastically decrease the fatigue performance of titanium alloys. The present work reports on the crystallographic orientation of a near-α titanium alloy, Ti60, billet after annealing in an α+β phase field. The texture was found to be weak, and no obvious macrozone was found in our measured zone where the variant selection is suppressed. Meanwhile, in-depth electron backscattered diffraction (EBSD) analysis was applied to evaluate the final microstructure, and the mechanisms by which they formed were analyzed.
WarwickJ L W, JonesN G, BantounasI, et al.
In situ observation of texture and microstructure evolution during rolling and globularization of Ti-6Al-4V
Analysis of the active slip mode during compression of the near-α titanium alloy in the α + β phase-field: Insights from the results of electron backscattered diffraction
Effects of strain state and slip mode on the texture evolution of a near-α TA15 titanium alloy during hot deformation based on crystal plasticity method
A thorough understanding of the texture evolution of near-α titanium alloys during the hot metal forming can help obtain an optimal crystallographic texture and material performance. The strain state has an obvious effect on the texture evolution of near-α titanium alloys during the hot metal forming. In this paper, the texture evolution of a near-α TA15 titanium alloy during the hot metal forming under different strain states were discussed based on the crystal plasticity finite element method. It is found that the basal and prismatic slip systems are regarded as the dominant slip modes due to the similar low critical resolved shear stress during the hot metal forming of the TA15 sheet rotating the lattice around the [10$\bar{1}$0] and 〈0001〉 axis, respectively. Once both of them cannot be activated, the pyramidal-2 slipping occurs rotating the lattice around the [10$\bar{1}$0] axis. The relationship between the texture evolution and strain state is established. All the (0001) orientations form a band perpendicular to the direction of the first principal strain. The width of the band along the direction of the second principal strain depends on the ratio of the compressive effect to the tensile effect of the second principal strain. This relationship can help control the crystallographic texture and mechanical properties of the titanium alloys component during the hot metal forming.
YooM H.
Slip, twinning, and fracture in hexagonal close-packed metals
The control of the post-forging cooling rate has been a key issue in the industrial production process of titanium alloys. We investigated texture evolution and variant selection (VS) during β → α transformation through high-temperature compression experiments followed by quantitative control of varying cooling rates. Results show that post-forging cooling rates affect β grains, α variants, and α / β textures. The α precipitation inhibits motions of β static recrystallization (βSRX) grain boundaries and thus leads to grain refining from 0.1 °C/s to 0.05 °C/s. Further analysis reveals that lamellae grain boundary widmanstatten α (αWGB) keeps growing rapidly within β-grain in an interface instability manner at 0.1-0.05 °C/s. Most of α-phase with 50°-60°/<-12-10> is preferentially precipitated at β-medium angle GBs between 30° and 45° and strictly follows BOR with the side of of adjacent β-grain with the same or similar {110} or {111}. Moreover, the texture type transforms gradually from RGoss {110} <1-10> to Brass {110} <1-12> from 25 °C/s to 1 °C/s. βSRX grains exhibit (102) [-201] texture, while the corresponding α has textures of <0001>//Z and <11-20>//Y from 1 °C/s to 0.05 °C/s. Our findings lay a profound theoretical foundation in microstructure evolution of near-β titanium alloy for industrial production.
FuruharaT, PoorganjiB, AbeH, et al.
Dynamic recovery and recrystallization in titanium alloys by hot deformation
Effect of microstructure on dwell fatigue behavior of Ti-6242
[A]. Proceedings of the Eighth World Conference on Titanium held at the International Convention Centre [C]. Birmingham: Institute of Materials, 1995: 1116
Correlation between imposed deformation and transformation lattice strain on α variant selection in a metastable β-Ti alloy under isothermal compression
... [14]Influences of hard-oriented primary α phase within macrozones on dwell-fatigue crack formation in titanium alloys[14] (a, c) SEM images showing the primary crack nucleation sites (b, d) crystallographic orientations relative to the loading direction in the same region (e) discrete pole figures (PFs) showing crystallographic orientations in locations numbered from 1 to 3 in Figs.1a and c (LD represents loading direction)Fig.1
... [14] (a, c) SEM images showing the primary crack nucleation sites (b, d) crystallographic orientations relative to the loading direction in the same region (e) discrete pole figures (PFs) showing crystallographic orientations in locations numbered from 1 to 3 in Figs.1a and c (LD represents loading direction)Fig.1
... [26,39]In-grain misorientation axis analysis (IGMA) based on EBSD orientation measurement for α colonies with different orientations in Ti60 alloy[26,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points) ...
... [26,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points) ...
... [26,45]Microstructures and crystallographic orientation evolutions of Ti60 alloy with α lamellae structure during thermal deformation at 900 oC (a, c, e) and 980 oC (b, d, f) (a, b) SEM images (Insets show enlarged SEM images)[45] (CD—compression direction) (c, d) IPF orientation maps (Insets show PFs of α texture measured by the XRD method)[45] (e, f) TEM bright field images[26,45]Fig.7
... [26,69]Evolutions of the αp/β phase boundary and its effects on microstructure during heat treatment of Ti60 alloy[26,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)Fig.9
... [26,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)Fig.9
... [26,39]In-grain misorientation axis analysis (IGMA) based on EBSD orientation measurement for α colonies with different orientations in Ti60 alloy[26,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points) ...
... [26,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points) ...
... [26,45]Microstructures and crystallographic orientation evolutions of Ti60 alloy with α lamellae structure during thermal deformation at 900 oC (a, c, e) and 980 oC (b, d, f) (a, b) SEM images (Insets show enlarged SEM images)[45] (CD—compression direction) (c, d) IPF orientation maps (Insets show PFs of α texture measured by the XRD method)[45] (e, f) TEM bright field images[26,45]Fig.7
... [26,69]Evolutions of the αp/β phase boundary and its effects on microstructure during heat treatment of Ti60 alloy[26,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)Fig.9
... [26,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)Fig.9
... [33]Effects of primary α phase on variant selection during β→α transformation and its contribution to texture intensity in macrozone[33] (a, c) inverse pole figures (IPFs) of specimens after compression (960 oC, 0.1 s-1, 30%) and then heat treatments at 980 oC (a) and 990 oC (c) for 1 h (TD, RD, and CA denotes transverse direction, radial direction, and compression axial direction, respectively) (b, d) IPFs and PFs of microtextured areas from Figs.3a and c (αp—primary α, αs—secondary α)Fig.3
... [33] (a, c) inverse pole figures (IPFs) of specimens after compression (960 oC, 0.1 s-1, 30%) and then heat treatments at 980 oC (a) and 990 oC (c) for 1 h (TD, RD, and CA denotes transverse direction, radial direction, and compression axial direction, respectively) (b, d) IPFs and PFs of microtextured areas from Figs.3a and c (αp—primary α, αs—secondary α)Fig.3
Analysis of the active slip mode during compression of the near-α titanium alloy in the α + β phase-field: Insights from the results of electron backscattered diffraction
... ,39]In-grain misorientation axis analysis (IGMA) based on EBSD orientation measurement for α colonies with different orientations in Ti60 alloy[26,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points) ...
... ,39]
(a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points) ...
... (a) IPF orientation maps(b) {0001} and {110} PFs (RD1 and RD2 represent radial directions 1 and 2, respectively)(c) IGMA distributions within 1°-5° of the selected A-D grains (The values indicated by the arrows represent the probabilities that the in-grain misorientation axis distributed near the c-axis. pts represent valid data points)Fig.5
热压缩变形过程中柱面<a>滑移系的开动及引起的晶格转动示意图[39]
Schematics showing the activation of prismatic <a> slip and induced lattice rotation during thermal compressed deformation[39]
(a) crystallography of the transformed α and matrix β phases in titanium alloys (a1-a3 denote the basal-plane lattice vectors of the hcp α-phase) ...
... [39]
(a) crystallography of the transformed α and matrix β phases in titanium alloys (a1-a3 denote the basal-plane lattice vectors of the hcp α-phase) ...
The origins of heterogeneous deformation during primary hot working of Ti-6Al-4V
... ,45]Microstructures and crystallographic orientation evolutions of Ti60 alloy with α lamellae structure during thermal deformation at 900 oC (a, c, e) and 980 oC (b, d, f) (a, b) SEM images (Insets show enlarged SEM images)[45] (CD—compression direction) (c, d) IPF orientation maps (Insets show PFs of α texture measured by the XRD method)[45] (e, f) TEM bright field images[26,45]Fig.7
... [45] (CD—compression direction) (c, d) IPF orientation maps (Insets show PFs of α texture measured by the XRD method)[45] (e, f) TEM bright field images[26,45]Fig.7
Effects of strain state and slip mode on the texture evolution of a near-α TA15 titanium alloy during hot deformation based on crystal plasticity method
0
2020
Slip, twinning, and fracture in hexagonal close-packed metals
... ,69]Evolutions of the αp/β phase boundary and its effects on microstructure during heat treatment of Ti60 alloy[26,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)Fig.9
... ,69] (a1, a2) Burgers orientation relationship (BOR) deviation angle (θ) distributions between αp grains and the neighboring β grains at 1030 oC (a1) and 1040 oC (a2) (fθ ≤ 10° denotes the number fraction of θ ≤ 10°)(b) band contrast (BC) map of αp grains with some special phase boundaries (GB—grain boundary)(c) schematic of β grain boundary (between grains A and B) pinning by an αp particle (particle C), showing the relevent interfacial energies (γAB, γAC, and γBC denote the interfacial energies of grains A and B, grain A and particle C, and grain B and particle C, respectively)Fig.9
Correlation between imposed deformation and transformation lattice strain on α variant selection in a metastable β-Ti alloy under isothermal compression